Integrated die casting release agent and preparation method thereof
Through the integrated die-casting release agent with specific ratios and process treatment, the problem of poor stability and release effect of traditional release agents in complex environments is solved, efficient lubrication and stability are achieved, and casting quality is improved. Mold life.
Patent Information
- Application Number
- CN202410559218.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-08
AI Technical Summary
Under the complex and changing die-casting environment and process requirements, traditional die-casting release agents are difficult to achieve ideal lubricity, demolding effect, thermal stability and chemical stability, resulting in poor surface quality of the casting and mold wear.
Using integrated die-casting release agent, including base oil with specific ratios, release active agents, metal passivating agents, stabilizers and anti-settling agents, the uniform and long-lasting process is formed through stirring, ultrasonic dispersion and pulsed magnetic field treatment. Lubricating film enhances the stability and release effect of the release agent.
It significantly improves the demolding efficiency and product quality, extends the service life of the demolding agent, reduces friction and adhesion, and ensures stable performance under high and low temperature conditions.
Smart Images

Figure BDA0004827051960000101 
Figure BDA0004827051960000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal casting, and in particular to an integrated die-casting release agent and a preparation method thereof. Background Art
[0002] Integrated die-casting release agent is a new type of release agent developed by the die-casting industry in recent years to meet the growing technical needs. Its research and development background mainly stems from the wide application of die-casting technology in multiple industries, especially in the rapid development of new energy vehicles, 5G communications, photovoltaics, energy storage and other fields, which puts forward higher requirements on the quality and performance of die-casting parts.
[0003] Although traditional die-casting release agents can meet basic demoulding requirements to a certain extent, their performance is often difficult to achieve ideal conditions when faced with complex and changeable die-casting environments and process requirements. In the integrated die-casting process, release agents play a vital role. They need to have excellent lubricity and demoulding effects to ensure that the die-casting can be smoothly separated from the mold, reduce mold wear, and improve the surface quality of the casting. For example, in terms of maintaining the fluidity of the alloy liquid, reducing mold cold and hot shocks, and improving demoulding efficiency, they need to have good thermal stability and chemical stability to adapt to high temperature and chemical corrosion working environments. Traditional release agents often perform poorly. Summary of the invention
[0004] In view of this, the present invention proposes an integrated die-casting release agent and a preparation method thereof to solve the above problems.
[0005] The technical solution of the present invention is achieved as follows: an integrated die-casting release agent comprises the following raw materials in parts by weight: 25-45 parts of base oil, 22-38 parts of a release agent, 10-15 parts of a metal passivator, 6-9 parts of a stabilizer, 8-10 parts of an anti-settling agent, and 5-10 parts of a bactericide, wherein the base oil comprises modified silicone oil, white oil, and vegetable oil in a mass ratio of (12-33):(8-10):(2-5); the vegetable oil is one of corn oil, rapeseed oil, bran oil, palm oil, cottonseed oil, sesame oil, safflower seed oil, soybean oil, sunflower seed oil, peanut oil, linseed oil, olive oil, rice oil, and tea seed oil, and the release agent comprises modified wax, sulfurized fatty acid ester, disulfide phosphate, and acetone in a mass ratio of (22-38):(12-34):(18-35):(3-8).
[0006] Furthermore, the following raw materials are included in parts by weight: 35 parts of base oil, 28 parts of mold release agent, 12 parts of metal passivator, 7 parts of stabilizer, 9 parts of anti-settling agent, and 8 parts of bactericide.
[0007] Furthermore, the modified silicone oil includes but is not limited to amino-modified silicone oil, epoxy-modified silicone oil, polyether-modified silicone oil, carboxyl-modified silicone oil, alcohol-hydroxyl-modified silicone oil, phenol-hydroxyl-modified silicone oil, mercapto-modified silicone oil, hydrogen silicone oil, ethyl silicone oil, phenyl silicone oil, chlorophenyl silicone oil, and trifluoropropyl silicone oil.
[0008] Furthermore, the modified wax is palm wax, Fischer-Tropsch wax, and maleated polyethylene wax in a mass ratio of (12-25):(8-10):(3-7).
[0009] Furthermore, the metal passivator includes but is not limited to benzotriazole sodium salt, organic stannate, triethyl antimony, cerium nitrate, lanthanum nitrate, phosphate, chromate, phosphate, and silicate.
[0010] Furthermore, the stabilizer is hydroquinone, 2,4-di-tert-butylphenyl, organic modified nano clay, and silicone polymer in a mass ratio of (6-8):(3-5):(0.8-1.5):(0.2-0.9); the organic modified nano clay is natural clay modified by an organic modifier, and the organic modifier is any one of hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, trimethoxysilane, trimethylphenylphosphonium iodide, and cocamidopropyl betaine, and the natural clay includes but is not limited to any one of bentonite, montmorillonite, kaolin, illite, sepiolite, rectorite, and talc; the silicone polymer is any one of polysiloxane, polysilane, polycarbosilane, and polynitrogen silane.
[0011] Furthermore, the anti-sedimentation agent is nanomagnetic beads, and the nanomagnetic beads are γ-Fe2O3 particles.
[0012] Furthermore, the bactericide includes any one or a combination of benzoic acid, sorbic acid, benzalkonium chloride, oxalic acid glycosides, and allyl isothiocyanate.
[0013] Furthermore, the preparation method of the integrated die-casting release agent comprises the following steps:
[0014] S1. Add base oil and mold release agent into the reaction kettle under stirring conditions, adjust the temperature to 60-80°C, mix thoroughly, gradually add metal passivator, and continue stirring until completely dispersed, with a stirring rate of 500-1000rpm to form a uniform solution;
[0015] S2. Disperse the above solution and stabilizer by ultrasonication, raise the temperature to 90-120°C under the protection of nitrogen, control the speed to 500-800 rpm and stir for 3-5 hours;
[0016] S3, adding an anti-settling agent on the basis of step S2, and subjecting the mixture to a pulsed magnetic field treatment for 5-30 minutes to obtain a mixture;
[0017] S4. Put the above mixture and fungicide into a high-speed disperser and disperse for 20-40 minutes. Adjust the power to 1.1-18.5 kW and the speed to 4800-5500 rpm.
[0018] Furthermore, the pulse frequency of the pulse magnetic field treatment of S3 is 1-25 Hz, the magnetic induction intensity is 0.5-3.5 T, and the pulse width is 200-300 ms.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The release agent of the present invention can form a uniform and lasting lubricating film during die casting through a specific raw material ratio and preparation process, effectively reducing the friction and adhesion between the mold and the casting, thereby improving the demoulding efficiency and product quality. A plurality of components such as base oil, demoulding activator and stabilizer in a specific ratio are selected, and these components work synergistically to form a stable and lasting lubricating film during die casting, significantly enhancing the stability and demoulding effect of the release agent, reducing the friction coefficient, and demoulding without grease, wax or other adhesive substances; by introducing stabilizers, such as organic modified nano clay and organosilicon polymers, the stability and durability of the release agent are enhanced, and a stable lubricating film can be maintained under high and low temperature change conditions, reducing the friction and adhesion between the mold and the casting; this helps to reduce the attenuation of the performance of the release agent during use and extend its service life; nano magnetic beads are used as anti-settling agents to effectively prevent the sedimentation of the release agent during storage and use, and ensure the uniformity and stability of the release agent.
[0021] The preparation method of the present invention is simple and clear, with clear steps, easy to operate and control, and is conducive to realizing industrial production. At the same time, by optimizing the preparation process, such as using ultrasonic dispersion and pulse magnetic field treatment, the microstructure and properties of the material surface can be changed, thereby improving the affinity and adhesion between the release agent and the mold surface, and improving the performance and quality of the release agent. DETAILED DESCRIPTION
[0022] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0023] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.
[0024] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0025] Example 1
[0026] The integrated die-casting release agent comprises the following raw materials in parts by weight: 25 parts of base oil, 22 parts of release activator, 10 parts of metal passivator, 6 parts of stabilizer, 8 parts of anti-settling agent, and 5 parts of bactericide;
[0027] The base oil includes amino-modified silicone oil, white oil and corn oil in a mass ratio of 12:8:2;
[0028] The demoulding active agent includes modified wax, sulfurized fatty acid ester, disulfide phosphate, and acetone in a mass ratio of 22:12:18:3; the modified wax is palm wax, Fischer-Tropsch wax, and maleated polyethylene wax in a mass ratio of 12:8:3;
[0029] The metal passivator is benzotriazole sodium salt;
[0030] The stabilizer is hydroquinone, 2,4-di-tert-butylphenyl, organic modified nano clay, and organosilicon polymer in a mass ratio of 6:3:0.8:0.2; the organic modified nano clay is natural clay modified by an organic modifier, the organic modifier is hexadecyltrimethylammonium chloride, and the natural clay is bentonite; the organosilicon polymer is polysiloxane;
[0031] The anti-settling agent is nanomagnetic beads, and the nanomagnetic beads are γ-Fe2O3 particles;
[0032] The bactericide is benzoic acid.
[0033] Example 2
[0034] The integrated die-casting release agent comprises the following raw materials in parts by weight: 45 parts of base oil, 38 parts of release activator, 15 parts of metal passivator, 9 parts of stabilizer, 10 parts of anti-settling agent, and 10 parts of bactericide;
[0035] The base oil includes epoxy-modified silicone oil, white oil and palm oil in a mass ratio of 33:10:5;
[0036] The demoulding active agent includes modified wax, sulfurized fatty acid ester, disulfide phosphate, and acetone in a mass ratio of 38:34:35:8; the modified wax is palm wax, Fischer-Tropsch wax, and maleated polyethylene wax in a mass ratio of 25:10:7;
[0037] The metal passivator is an organic stannate;
[0038] The stabilizer is hydroquinone, 2,4-di-tert-butylphenyl, organic modified nano clay, and organosilicon polymer in a mass ratio of 8:5:1.5:0.9; the organic modified nano clay is obtained by modifying natural clay with an organic modifier, the organic modifier is hexadecyltrimethylammonium bromide, and the natural clay is kaolin; the organosilicon polymer is polysilane;
[0039] The anti-settling agent is nanomagnetic beads, and the nanomagnetic beads are γ-Fe2O3 particles;
[0040] The bactericide is benzalkonium chloride.
[0041] Example 3
[0042] The integrated die-casting release agent comprises the following raw materials in parts by weight: 35 parts of base oil, 28 parts of release activator, 12 parts of metal passivator, 7 parts of stabilizer, 9 parts of anti-settling agent, and 8 parts of bactericide;
[0043] The base oil includes polyether-modified silicone oil, white oil and bran oil in a mass ratio of 22:9:3;
[0044] The demoulding active agent includes modified wax, sulfurized fatty acid ester, disulfide phosphate, and acetone in a mass ratio of 30:23:28:5; the modified wax is palm wax, Fischer-Tropsch wax, and maleated polyethylene wax in a mass ratio of 18:9:5;
[0045] The metal passivator is triethyl antimony;
[0046] The stabilizer is hydroquinone, 2,4-di-tert-butylphenyl, organic modified nano clay, and organosilicon polymer in a mass ratio of 7:4:1.2:0.7; the organic modified nano clay is obtained by modifying natural clay with an organic modifier, the organic modifier is trimethoxysilane, and the natural clay is kaolin; the organosilicon polymer is polycarbosilane;
[0047] The anti-settling agent is nanomagnetic beads, and the nanomagnetic beads are γ-Fe2O3 particles;
[0048] The bactericide is benzoic acid.
[0049] The above examples 1-3 adopt the following preparation method:
[0050] S1. Add base oil and mold release agent into the reactor under stirring conditions, adjust the temperature to 70°C, mix thoroughly, gradually add metal passivator, and continue stirring until completely dispersed, with a stirring rate of 800 rpm to form a uniform solution;
[0051] S2. Disperse the above solution and stabilizer by ultrasonication, raise the temperature to 110° C. under the protection of nitrogen, control the speed to 700 rpm and stir for 4 h;
[0052] S3, adding an anti-settling agent on the basis of step S2, and subjecting to pulsed magnetic field treatment for 17 minutes, with a pulse frequency of 12 Hz, a magnetic induction intensity of 2.0 T, and a pulse width of 250 ms, to obtain a mixture after treatment;
[0053] S4. Put the above mixture and fungicide into a high-speed disperser and disperse for 30 minutes. Adjust the power to 9.5 kW and the speed to 5200 rpm.
[0054] Example 4
[0055] The integrated die-casting release agent comprises the following raw materials in parts by weight: 35 parts of base oil, 28 parts of release activator, 12 parts of metal passivator, 7 parts of stabilizer, 9 parts of anti-settling agent, and 8 parts of bactericide;
[0056] The base oil includes polyether-modified silicone oil, white oil and bran oil in a mass ratio of 22:9:3;
[0057] The demoulding active agent includes modified wax, sulfurized fatty acid ester, disulfide phosphate, and acetone in a mass ratio of 30:23:28:5; the modified wax is palm wax, Fischer-Tropsch wax, and maleated polyethylene wax in a mass ratio of 18:9:5;
[0058] The metal passivator is triethyl antimony;
[0059] The stabilizer is hydroquinone, 2,4-di-tert-butylphenyl, organic modified nano clay, and organosilicon polymer in a mass ratio of 7:4:1.2:0.7; the organic modified nano clay is obtained by modifying natural clay with an organic modifier, the organic modifier is trimethoxysilane, and the natural clay is kaolin; the organosilicon polymer is polycarbosilane;
[0060] The anti-settling agent is nanomagnetic beads, and the nanomagnetic beads are γ-Fe2O3 particles;
[0061] The bactericide is benzoic acid.
[0062] The above-mentioned Example 4 adopts the following preparation method:
[0063] S1. Add base oil and release agent into the reaction kettle under stirring conditions, adjust the temperature to 60°C, mix thoroughly, gradually add metal passivator, and continue stirring until completely dispersed, with a stirring rate of 500 rpm to form a uniform solution;
[0064] S2. Disperse the above solution and stabilizer by ultrasonication, raise the temperature to 90°C under the protection of nitrogen, and stir at a speed of 500 rpm for 3 hours;
[0065] S3, adding an anti-settling agent on the basis of step S2, and subjecting to a pulsed magnetic field treatment for 5 min, with a pulse frequency of 1 Hz, a magnetic induction intensity of 0.5 T, and a pulse width of 200 ms, to obtain a mixture after treatment;
[0066] S4. Put the above mixture and fungicide into a high-speed disperser and disperse for 20 minutes. Adjust the power to 1.1kW and the speed to 4800rpm.
[0067] Example 5
[0068] The integrated die-casting release agent comprises the following raw materials in parts by weight: 35 parts of base oil, 28 parts of release activator, 12 parts of metal passivator, 7 parts of stabilizer, 9 parts of anti-settling agent, and 8 parts of bactericide;
[0069] The base oil includes polyether-modified silicone oil, white oil and bran oil in a mass ratio of 22:9:3;
[0070] The demoulding active agent includes modified wax, sulfurized fatty acid ester, disulfide phosphate, and acetone in a mass ratio of 30:23:28:5; the modified wax is palm wax, Fischer-Tropsch wax, and maleated polyethylene wax in a mass ratio of 18:9:5;
[0071] The metal passivator is triethyl antimony;
[0072] The stabilizer is hydroquinone, 2,4-di-tert-butylphenyl, organic modified nano clay, and organosilicon polymer in a mass ratio of 7:4:1.2:0.7; the organic modified nano clay is obtained by modifying natural clay with an organic modifier, the organic modifier is trimethoxysilane, and the natural clay is kaolin; the organosilicon polymer is polycarbosilane;
[0073] The anti-settling agent is nanomagnetic beads, and the nanomagnetic beads are γ-Fe2O3 particles;
[0074] The bactericide is benzoic acid.
[0075] The above-mentioned Example 5 adopts the following preparation method:
[0076] S1. Add the base oil and the release agent into the reaction kettle under stirring conditions, adjust the temperature to 80°C, mix thoroughly, gradually add the metal passivator, and continue stirring until it is completely dispersed. The stirring rate is 1000 rpm to form a uniform solution.
[0077] S2. The above solution and stabilizer are dispersed by ultrasonic, and the temperature is raised to 120° C. under the protection of nitrogen, and the speed is controlled to 800 rpm for stirring for 5 hours;
[0078] S3, adding an anti-settling agent on the basis of step S2, and subjecting to a pulsed magnetic field treatment for 30 min, with a pulse frequency of 25 Hz, a magnetic induction intensity of 3.5 T, and a pulse width of 300 ms, to obtain a mixture after treatment;
[0079] S4. Put the above mixture and fungicide into a high-speed disperser for 40 minutes, adjust the power to 18.5kW and the speed to 5500rpm.
[0080] Comparative Example 1
[0081] The difference between this comparative example and Example 3 is that the integrated die-casting release agent includes the following raw materials in parts by weight: 65 parts of base oil, 58 parts of release activator, 5 parts of metal passivator, 2 parts of stabilizer, 5 parts of anti-settling agent, and 2 parts of bactericide.
[0082] Comparative Example 2
[0083] The difference between this comparative example and Example 3 is that the base oil in the raw material of the integrated die-casting release agent is an equal amount of silicone oil.
[0084] Comparative Example 3
[0085] The difference between this comparative example and Example 3 is that the demoulding active agent in the raw materials of the integrated die-casting demoulding agent is palm wax, Fischer-Tropsch wax, and maleated polyethylene wax in a mass ratio of 18:9:5.
[0086] Comparative Example 4
[0087] The difference between this comparative example and Example 3 is that the raw material of the integrated die-casting release agent does not contain an anti-settling agent.
[0088] Comparative Example 5
[0089] The difference between this comparative example and Example 3 is that the pulsed magnetic field treatment step is not performed in the preparation method of the integrated die-casting release agent, specifically:
[0090] S1. Add base oil and mold release agent into the reactor under stirring conditions, adjust the temperature to 70°C, mix thoroughly, gradually add metal passivator, and continue stirring until completely dispersed, with a stirring rate of 800 rpm to form a uniform solution;
[0091] S2. Disperse the above solution and stabilizer by ultrasonication, raise the temperature to 110° C. under the protection of nitrogen, control the speed to 700 rpm and stir for 4 h;
[0092] S3. Put the above mixture, anti-settling agent and bactericide into a high-speed disperser and disperse for 30 minutes. Adjust the power to 9.5 kW and the speed to 5200 rpm.
[0093] 1. Performance Testing
[0094] Set up 10 groups of tests, corresponding to the above-mentioned Examples 1-5 and Comparative Examples 1-5 and commercially available release agents, and test the friction coefficient, residue, and stability thereof, with three parallel tests in each group;
[0095] (1) Friction coefficient test: Apply the above release agent to the test area of the aluminum alloy substrate. The amount of release agent is 2.0 mg / cm 2 , use a die pressing device to press and form, the pressure is 35T, leave it for 48 hours, place the test surface in the corresponding position of the friction coefficient tester, and ensure that the contact pressure of 5N is evenly distributed;
[0096] (2) Residue detection: Observe the product surface under sufficient light;
[0097] The test results are shown in Table 1:
[0098] Friction coefficient Residue Example 1 0.15 No grease, wax or other sticky substances Example 2 0.13 No grease, wax or other sticky substances Example 3 0.12 No grease, wax or other sticky substances Example 4 0.19 No grease, wax or other sticky substances Example 5 0.18 No grease, wax or other sticky substances Comparative Example 1 0.22 Small localized accumulation of grease and wax Comparative Example 2 0.25 Local accumulation of grease, wax, and granular residues Comparative Example 3 0.26 Grease, wax and granular residues are evenly distributed Comparative Example 4 0.28 Grease, wax, and granular residues are loosely attached and distributed Comparative Example 5 0.31 Grease, wax, and granular residues are loosely attached and distributed Commercially available 0.54 Grease, wax, and granular residues are tightly attached and distributed
[0099] From the above results, it can be seen that compared with the commercially available release agent, the release agent of the present invention has better demoulding efficiency, and the friction coefficient of Examples 1-5 is less than 0.2;
[0100] Compared with comparative example 1, the embodiment group can ensure that the release agent forms a uniform and stable film on the mold surface by precisely controlling the proportion of the release agent raw materials. This film can effectively reduce the friction between the mold and the product, so that the product can be more easily separated from the mold and the demolding efficiency is improved.
[0101] Compared with the comparative example 2, the base oil configured in the embodiment group of the present invention, through the reasonable proportion of modified silicone oil, white oil and vegetable oil, can penetrate into the tiny gaps on the surface of the mold, can adjust the viscosity, adhesion and stability of the release agent, enhance the bonding force between the release agent and the mold surface, and improve the demoulding effect;
[0102] Compared with the comparative example 3, the demoulding active agent configured in the embodiment group of the present invention can help the metal demoulding agent to be better coated on the mold surface and form a uniform isolation film on the mold surface. This film can reduce the adhesion between the metal and the mold, so that the metal parts can be easily separated from the mold; wherein, the modified wax improves the adhesion to the metal surface through chemical modification, provides a good demoulding effect, and has good thermal stability and low melting point, can form a uniform protective film on the mold surface, and reduce mold wear; the sulfided fatty acid ester forms a stable sulfur compound film on the mold surface, improves the chemical stability of the demoulding agent, reduces the reaction with other components, and prolongs the service life of the demoulding agent; the disulfide phosphate forms an anti-adhesion inorganic film on the surface, which improves the wear resistance and bearing capacity of the demoulding agent; acetone, as a solvent or diluent in the demoulding agent, can reduce the viscosity of the demoulding agent, improve its spreadability and wettability on the mold surface, and due to the volatility of acetone, it helps the demoulding agent to dry quickly, forms a uniform film on the mold surface, and reduces the residue of the demoulding agent;
[0103] Compared with comparative example 4, the embodiment group uses γ-Fe2O3 particles as anti-settling agents, which have superparamagnetism and can quickly aggregate under the action of an external magnetic field and disperse evenly after removing the magnetic field. This helps to maintain the suspension state of the solid particles in the release agent and prevent them from settling. It can also fill the tiny bumps on the mold surface and can be evenly dispersed in the release agent to form a stable suspension system, which facilitates better demolding.
[0104] Compared with Example 5, the embodiment group shows that the pulsed magnetic field treatment of the mixed liquid can change the microstructure and properties of the material surface, thereby improving the affinity and adhesion between the release agent and the mold surface, improving the dispersibility and stability of each component in the release agent, reducing sedimentation and stratification, and maintaining the uniformity and long-term effectiveness of the release agent.
[0105] (3) Stability test:
[0106] Comparative Example 6
[0107] The difference between this comparative example and Example 3 is that the raw materials of the integrated die-casting release agent contain dibutyltin dilaurate, dibutyltin dimaleate, and zinc stearate in a mass ratio of 1:1:1.
[0108] The release agent samples of Example 3 and Comparative Examples 1, 4-6 were heated to 80°C, and then cooled to 5°C, and their viscosity change rates were tested;
[0109] Viscosity change rate (%) = (viscosity at the end of the experiment - initial viscosity) / initial viscosity × 100%;
[0110] The test results are shown in Table 2:
[0111]
[0112]
[0113] Note: The above values are absolute values
[0114] It can be seen from the above stability results that the release agent of the present invention has good stability and has a small viscosity change rate at temperatures of 80°C and 5°C. The stabilizer configured in the present invention has strong stability. Hydroquinone can be used as an antioxidant to help improve the stability of the metal release agent and prevent it from oxidative degradation during temperature changes or long-term storage. 2,4-di-tert-butylphenyl can improve the stability of the release agent and reduce performance fluctuations caused by temperature changes. Organically modified nanoclay, as a filler, has a very high specific surface area and adsorption performance, which can improve the viscosity and rheological properties of the release agent, enhance the lubricity and adhesion of the release agent at high and low temperatures, and ensure that the demolding effect is not affected by temperature. The organosilicon polymer has excellent low-temperature fluidity and lubricity. Under high and low temperature conditions, the organosilicon polymer can maintain a stable lubricating film, reduce friction and adhesion between the mold and the casting, thereby improving the demolding efficiency and reducing product damage; the four components work synergistically to improve the stability, high temperature resistance, lubrication effect and demolding efficiency of the metal release agent;
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. Integrated die casting release agent, characterized by: The invention comprises the following raw materials in parts by weight: 25-45 parts of base oil, 22-38 parts of demoulding active agent, 10-15 parts of metal passivator, 6-9 parts of stabilizer, 8-10 parts of anti-settling agent and 5-10 parts of bactericide, wherein the base oil comprises modified silicone oil, white oil and vegetable oil in a mass ratio of (12-33):(8-10):(2-5); the demoulding active agent comprises modified wax, sulfurized fatty acid ester, disulfide phosphate and acetone in a mass ratio of (22-38):(12-34):(18-35):(3-8); The modified wax is palm wax, Fischer-Tropsch wax, and maleated polyethylene wax in a mass ratio of (12-25):(8-10):(3-7); The stabilizer is hydroquinone, 2,4-di-tert-butylbenzene, organic modified nano clay, and organic silicon polymer in a mass ratio of (6-8):(3-5):(0.8-1.5):(0.2-0.9); the organic modified nano clay is obtained by modifying natural clay with an organic modifier, the organic modifier is any one of hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, trimethoxysilane, trimethylphenylphosphonium iodide, and cocamidopropyl betaine, the natural clay includes any one of bentonite, montmorillonite, kaolin, illite, sepiolite, rectorite, and talc; the organic silicon polymer is any one of polysiloxane, polysilane, polycarbosilane, and polynitrogen silane.
2. The integrated die-casting release agent according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 35 parts of base oil, 28 parts of demoulding active agent, 12 parts of metal passivator, 7 parts of stabilizer, 9 parts of anti-settling agent and 8 parts of bactericide.
3. The integrated die-casting release agent according to claim 1, characterized in that: The modified silicone oil includes amino-modified silicone oil, epoxy-modified silicone oil, polyether-modified silicone oil, carboxyl-modified silicone oil, alcohol-hydroxyl-modified silicone oil, phenol-hydroxyl-modified silicone oil, mercapto-modified silicone oil, hydrogen silicone oil, ethyl silicone oil, phenyl silicone oil, chlorophenyl silicone oil, and trifluoropropyl silicone oil.
4. The integrated die-casting release agent according to claim 1, characterized in that: The metal passivator includes benzotriazole sodium salt, organic stannate, triethyl antimony, cerium nitrate, lanthanum nitrate, phosphate, chromate, and silicate.
5. The integrated die-casting release agent according to claim 1, characterized in that: The anti-sedimentation agent is nano-magnetic beads, and the nano-magnetic beads are γ-Fe2O3 particles.
6. The integrated die-casting release agent according to claim 1, characterized in that: The bactericide includes any one or a combination of benzoic acid, sorbic acid, benzalkonium chloride, glycyrrhizic acid, and allyl isothiocyanate.
7. The method for preparing the integrated die-casting release agent according to claim 1, characterized in that: The following steps are involved: S1. Add base oil and mold release agent into the reaction kettle under stirring conditions, adjust the temperature to 60-80°C, mix thoroughly, gradually add metal passivator, and continue stirring until completely dispersed, with a stirring rate of 500-1000rpm to form a uniform solution; S2. Disperse the above solution and stabilizer by ultrasonication, raise the temperature to 90-120°C under the protection of nitrogen, control the speed to 500-800 rpm and stir for 3-5 hours; S3, adding an anti-settling agent on the basis of step S2, and subjecting the mixture to a pulsed magnetic field treatment for 5-30 minutes to obtain a mixture; S4. Put the above mixture and fungicide into a high-speed disperser and disperse for 20-40 minutes. Adjust the power to 1.1-18.5 kW and the speed to 4800-5500 rpm.