An electrocatalytic anode material for treating organic wastewater and its preparation method and application

The acid-base-resistant electrocatalytic anode is prepared by reacting inexpensive catalyst support and transition metal salt at high temperatures, solving the problems of low efficiency and secondary pollution in the prior art, and achieving efficient and applicable electrocatalytic oxidation treatment effect .

CN118515344BActive Publication Date: 2024-11-26HUNAN INSTITUTE OF ENGINEERING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966215.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-26
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The prior art is inefficient and produces secondary pollution when dealing with complex organic wastewater, and has a shortage of high-efficiency electrocatalytic anode materials, limiting the large-scale application of electrocatalytic oxidation in the industry.

Method used

The electrocatalytic anode is prepared by reacting inexpensive catalyst support with transition metal salt at high temperature. Combined with alkaline treatment and acid washing, it forms an electrocatalytic plate that is resistant to acid and alkali corrosion and has high conductivity, and is used for electrocatalytic oxidation of low-concentration organic wastewater deal with.

Benefits of technology

It has achieved efficient oxidation treatment of low-concentration organic wastewater, with a treatment efficiency of up to 84.8%, is not affected by pH, is suitable for a variety of water bodies, has high efficiency in degradation of COD, and has a wide selection of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides an electrocatalytic anode material for treating organic wastewater and a preparation method and application thereof, belonging to the technical field of chemically modified electrodes for treating wastewater by electrocatalytic oxidation. The selected carrier material skeleton is activated carbon, graphite and foamed metal after alkali treatment. During preparation, one or more metal salts are first prepared into a stable aqueous solution, mixed with the carrier material in a certain proportion and soaked for a certain time, so that the carrier material fully absorbs the metal salt solution, and then the absorbed composite is dried and dehydrated, and then the metal salt and the carrier material are subjected to high temperature to chemically react to generate a stable composite, and then washed with an acidic aqueous solution to obtain the electrocatalytic anode material; the metal salt and the carrier or the metal salt and the metal salt are subjected to high temperature sintering to chemically react to generate a stable electrocatalytic anode material, and a class of electrocatalytic anode materials with large metal loading and high catalytic efficiency are obtained by pretreating the conductive substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemically modified electrodes for treating wastewater by electrocatalytic oxidation, and specifically relates to an electrocatalytic anode material for treating organic wastewater, and a preparation method and application thereof. Background Art

[0002] The treatment of industrial organic wastewater is a major problem faced in pharmaceutical and chemical production. The pollutant composition of this type of wastewater is relatively complex, and the content of various substances in the water body varies greatly. There are many problems in the treatment process of this type of wastewater. If this type of wastewater is not treated properly or is not treated up to standard, it will not only affect industrial production, but also seriously pollute the ecological environment. Therefore, it is necessary to develop new catalysts for the treatment of organic wastewater.

[0003] At present, the main methods for treating organic wastewater are Fenton oxidation, wet oxidation, biochemical method, physical adsorption, electrocatalytic oxidation, and photocatalytic oxidation. Although these methods have been widely used in industry, they still face many problems. Fenton oxidation is the most common method. Although this method has certain cost advantages in treating high-concentration organic wastewater, its efficiency in treating complex organic wastewater is not high, and it will also produce a large amount of secondary pollutants such as iron mud. The large amount of sulfate introduced during the treatment process will also produce sulfur-containing toxic gases such as hydrogen sulfide in the subsequent biochemical treatment. Although the wet oxidation method has a high treatment efficiency, the treatment conditions are strict, which is not only costly but also has certain safety hazards. Although the biochemical method has a low cost in treating organic wastewater, complex organic wastewater must be pretreated before entering the biochemical system, and the biochemical treatment efficiency of complex organic matter is low. Although the electrocatalytic oxidation method is simple to treat and has no secondary pollution, the anode materials that can be selected are relatively limited. The shortage of high-efficiency electrocatalytic anode materials limits the large-scale application of this method in industry.

[0004] Therefore, it is necessary to develop efficient electrocatalytic plates for electrocatalytic oxidation treatment of organic wastewater. Currently, most electrocatalytic anodes used in the market are titanium dioxide series coating materials, which are highly efficient but expensive. In the present invention, a cheap catalyst carrier is used to prepare an efficient electrocatalytic anode for oxidation treatment of low-concentration organic wastewater by compounding common transition metal salts, which can treat low-concentration organic wastewater to meet surface water discharge requirements. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an electrocatalytic anode material for treating organic wastewater, and a preparation method and application thereof, wherein one or more metal salts react with a carrier material at high temperature to combine them in the form of chemical bonds to prepare an electrocatalytic plate for electrocatalytic oxidation treatment of low-concentration organic wastewater. The electrocatalytic anode prepared by this method has strong acid and alkali corrosion resistance, high electrical conductivity, and high electrocatalytic oxidation efficiency. Combined with the use of an external oxidant, low-concentration organic wastewater can be efficiently electrocatalytically oxidized.

[0006] To achieve the above object, the present invention first provides a method for preparing an electrocatalytic anode material for treating organic wastewater, comprising the following steps:

[0007] S1, soaking the highly conductive substrate in an alkaline solution, drying it in an oven, and heating it to 300° C. in a tube furnace under an inert gas atmosphere to obtain a carrier material, which is then kept warm for later use;

[0008] S2, immersing the carrier material prepared in S1 in an aqueous solution of a metal salt for adsorption loading, and placing the adsorbed carrier material

[0009] Place in an oven to dry, then place in a tube furnace under an inert gas atmosphere and heat to 500-1000°C for insulation;

[0010] S3, washing the support material obtained in S2 with an acidic solution to obtain an electrocatalytic anode material;

[0011] The highly conductive substrate in step S1 is selected from any one of activated carbon, graphite, and foamed metal;

[0012] The alkaline solution in step S1 is selected from any one of sodium hydroxide solution, potassium hydroxide solution, sodium carbonate solution, and potassium phosphate solution;

[0013] The metal salt in step S2 includes one or more of transition metal or noble metal chlorides, transition metal or noble metal sulfates, transition metal or noble metal nitrates, and transition metal or noble metal acetates.

[0014] Preferably, the activated carbon is selected from any one of coconut shell activated carbon, wood activated carbon, fruit shell activated carbon, and coal activated carbon; the graphite is selected from any one of block graphite and flake graphite; the foam metal is selected from any one of foam nickel, foam copper, and foam titanium.

[0015] Preferably, the drying temperature in step S1 is 80° C., the drying time is 2 h, the inert gas is selected from nitrogen or argon; the heating rate is 5° C. / min; and the insulation time is 4 h.

[0016] Preferably, the transition metal includes one of iron, cobalt, nickel, copper and zinc, and the noble metal includes one of gold, silver, palladium and platinum.

[0017] Preferably, in step S2, the mass of the metal salt is 5-20% of the carrier material, and the concentration of the aqueous solution of the metal salt is 2-10%.

[0018] Preferably, the adsorption load time in step S2 is 4 hours; the drying temperature is 80-300°C, and the drying time is 2-4 hours; the inert gas is selected from nitrogen or argon; the heating rate is 5°C / min; and the insulation time is 4-8 hours.

[0019] Preferably, the acidic solution in step S3 includes one of citric acid solution, oxalic acid solution, acetic acid solution, hydrochloric acid solution and hydrofluoric acid solution.

[0020] Based on a general inventive concept, the present invention provides an electrocatalytic anode material for treating organic wastewater prepared by the above-mentioned preparation method.

[0021] Based on a general inventive concept, the present invention provides an application of an electrocatalytic anode material for treating organic wastewater in treating low COD organic wastewater. The application method is: placing the electrocatalytic anode material into 100-200 mg / L low COD organic wastewater, using a metal plate as the cathode, with an electrode spacing of 2-50 mm, a voltage of 4-12 V, and electrocatalytic oxidation for 0.5 h.

[0022] Preferably, the metal plate includes one of a titanium plate and an iron plate.

[0023] The mechanism of catalytic oxidation treatment of low COD organic wastewater in this scheme is as follows:

[0024] In this scheme, the highly conductive substrate is treated with an alkaline solution. The alkaline solution will cause the carrier surface to have more hydroxyl groups. The presence of hydroxyl groups will be more conducive to the adsorption and loading of metal particles. First, the metal salt is adsorbed and loaded on the highly conductive substrate, and then a chemical reaction is caused between the metal salt and the carrier or between the metal salt and the metal salt by high-temperature sintering to generate a stable electrocatalytic anode material. By pretreating the conductive substrate, a type of electrocatalytic anode material with a large metal loading and high catalytic efficiency is obtained.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) This scheme prepares an electrocatalytic anode material for treating organic wastewater, which can be directly used as an anode material to catalyze the oxidation of organic wastewater. The preparation method is simple and the COD degradation efficiency is high.

[0027] (2) The anode material prepared by this scheme is not affected by pH when treating low-COD organic wastewater and is suitable for a variety of water bodies with different pH values. The efficiency can reach up to 84.8% in actual wastewater treatment.

[0028] (3) The electrocatalytic anode material for treating organic wastewater prepared by this scheme has a variety of optional carrier materials. The metal salts include metal chlorides, metal sulfates, metal acetates and metal acetates. The raw material range is wide and the selectivity is high. DETAILED DESCRIPTION

[0029] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, they are described in detail below in conjunction with specific embodiments.

[0030] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Without departing from the spirit and substance of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.

[0031] Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art; unless otherwise specified, the reagents used in the examples are commercially available.

[0032] Example 1 Preparation of electrocatalytic anode material for treating organic wastewater.

[0033] S1, 0.01m 2 The block graphite felt (weight 10g) was first soaked in a 2% sodium hydroxide aqueous solution for four hours, and after draining the water, it was placed in an 80°C oven for 2 hours, and then placed in a tubular furnace under a nitrogen atmosphere and heated to 300°C at a rate of 5°C / min, and kept warm for 4 hours for use.

[0034] S2. Prepare 300 ml of aqueous solution with a metal ion content of 5% by mixing copper chloride, cobalt chloride and nickel chloride in a mass ratio of 1:1:1, and soak the pretreated graphite felt in the metal salt solution for 4 hours. After the graphite felt is saturated with adsorption, dry it in an oven at 80°C for 2 hours, and then place it in a tubular furnace under a nitrogen atmosphere and heat it to 800°C at a rate of 5°C / min, and keep it warm for 8 hours.

[0035] S3. Wash with citric acid solution to obtain the electrocatalytic anode.

[0036] Example 2 Preparation of electrocatalytic anode material for treating organic wastewater.

[0037] S1, 0.01m 2The block graphite felt (weight 10g) was first soaked in a 2% sodium hydroxide aqueous solution for four hours, and after draining the water, it was placed in an 80°C oven for 2 hours, and then placed in a tubular furnace under a nitrogen atmosphere and heated to 300°C at a rate of 5°C / min, and kept warm for 4 hours for use.

[0038] S2. Prepare 300 ml of an aqueous solution with a metal ion content of 5% by weight of copper chloride and cobalt chloride in a mass ratio of 1:1, and soak the pretreated graphite felt in the metal salt solution for 4 hours. After the graphite felt is saturated with adsorption, dry the graphite felt after adsorbing the metal salt solution in an oven at 80°C for 2 hours, and then place it in a tubular furnace under a nitrogen atmosphere and heat it to 800°C at a rate of 5°C / min, and keep it warm for 8 hours.

[0039] S3. Wash with citric acid solution to obtain the electrocatalytic anode.

[0040] Example 3 Preparation of electrocatalytic anode material for treating organic wastewater.

[0041] S1, 0.01m 2 The block graphite felt (weight 10g) was first soaked in a 2% potassium hydroxide aqueous solution for four hours, and after draining the water, it was placed in an 80℃ oven for 2 hours, and then placed in a tubular furnace under an argon atmosphere and heated to 300℃ at a rate of 5℃ / min, and kept warm for 4 hours for use.

[0042] S2. Prepare 300 ml of an aqueous solution with a metal ion content of 5% by weight of copper chloride, cobalt chloride and nickel chloride in a mass ratio of 1:2:1, and soak the pretreated graphite felt in the metal salt solution for 4 hours. After the graphite felt is saturated with adsorption, dry the graphite felt after adsorbing the metal salt solution in an oven at 80°C for 2 hours, and then place it in a tubular furnace under a nitrogen atmosphere and heat it to 500°C at a rate of 5°C / min, and keep it warm for 8 hours.

[0043] S3. Wash with oxalic acid solution to obtain the electrocatalytic anode.

[0044] Example 4 Preparation of electrocatalytic anode material for treating organic wastewater.

[0045] S1, 0.01m 2 Coconut shell activated carbon sheets (weight 8g) were first soaked in 2% sodium hydroxide aqueous solution for four hours, drained and dried in an oven at 80°C for 2 hours, then placed in a tubular furnace under a nitrogen atmosphere and heated to 300°C at a rate of 5°C / min, and kept warm for 4 hours for use.

[0046] S2, tin chloride, lead nitrate, potassium chloroplatinate according to the mass ratio of 1:2:1 to prepare 300 ml of aqueous solution with a metal ion content of 5%, the pretreated coconut shell activated carbon sheet is placed in the metal salt solution and soaked for 4 hours, after the coconut shell activated carbon sheet is saturated with adsorption, the coconut shell activated carbon sheet after adsorption of the metal salt solution is placed in an oven at 80°C for 2 hours, and then placed in a tubular furnace under a nitrogen atmosphere at a heating rate of 5°C / min to 1000°C, and kept warm for 8 hours;

[0047] S3. Wash with citric acid solution to obtain the electrocatalytic anode.

[0048] Example 5 Preparation of electrocatalytic anode material for treating organic wastewater.

[0049] S1, 0.01m 2 The foam copper plate (weight 15g) was first soaked in sodium carbonate solution for four hours, drained and dried in an oven at 80℃ for 2 hours, then placed in a tubular furnace under argon atmosphere and heated to 300℃ at a rate of 5℃ / min, and kept warm for 4 hours for use.

[0050] S2, tin chloride, lead sulfate, potassium chloropalladate according to the mass ratio of 1:2:1 to prepare 300 ml of aqueous solution with a metal ion content of 5%, the pretreated foam copper plate is placed in the metal salt solution and soaked for 4 hours, after the foam copper plate is saturated with adsorption, the foam copper plate after adsorption of the metal salt solution is placed in an oven at 80°C for 2 hours, and then placed in a tubular furnace under a nitrogen atmosphere at a heating rate of 5°C / min to 1000°C, and kept warm for 8 hours;

[0051] S3. Wash with acetic acid solution to obtain the electrocatalytic anode.

[0052] Example 6 Preparation of electrocatalytic anode material for treating organic wastewater.

[0053] S1, 0.01m 2 The foam titanium plate (weight 12g) was first soaked in sodium carbonate solution for four hours, and then dried in an 80°C oven for 2 hours after draining the water. It was then placed in a tubular furnace under an argon atmosphere and heated to 300°C at a rate of 5°C / min, and kept warm for 4 hours for use.

[0054] S2, copper nitrate, lead sulfate, potassium chloropalladate according to the mass ratio of 1:2:1 to prepare 300 ml of aqueous solution with a metal ion content of 5%, the pretreated titanium foam plate is placed in the metal salt solution and soaked for 4 hours, after the titanium foam plate is saturated with adsorption, the titanium foam plate after adsorption of the metal salt solution is placed in an oven at 80°C for 2 hours, and then placed in a tubular furnace under a nitrogen atmosphere at a heating rate of 5°C / min to 1000°C, and kept warm for 8 hours;

[0055] S3. Wash with acetic acid solution to obtain the electrocatalytic anode.

[0056] Comparative Example 1 Preparation of electrocatalytic anode material without alkali pretreatment.

[0057] S1, 0.01m 2 A block of graphite felt (weight 10 g) was placed in a tubular furnace under a nitrogen atmosphere and heated to 300°C at a rate of 5°C / min, and kept at this temperature for 4 hours for later use;

[0058] S2. Prepare 300 ml of aqueous solution with a metal ion content of 5% by mixing copper chloride, cobalt chloride and nickel chloride in a mass ratio of 1:1:1, and soak the above graphite felt in the metal salt solution for 4 hours. After the graphite sheet is saturated with adsorption, place the graphite felt after adsorbing the metal salt solution in an oven at 80°C for 2 hours, and then place it in a tubular furnace under a nitrogen atmosphere and heat it to 800°C at a rate of 5°C / min, and keep it warm for 8 hours.

[0059] S3. Wash with citric acid solution to obtain the electrocatalytic anode.

[0060] Comparative Example 2 Preparation of an electrocatalytic anode material without metal salt.

[0061] S1, 0.01m 2 The foam titanium plate (weight 12g) was first soaked in sodium carbonate solution for four hours, and then dried in an 80°C oven for 2 hours after draining the water. It was then placed in a tubular furnace under an argon atmosphere and heated to 300°C at a rate of 5°C / min, and kept warm for 4 hours for use.

[0062] S2, drying the titanium foam plate in an oven at 80°C for 2 hours, and then placing the plate in a tubular furnace under a nitrogen atmosphere at a heating rate of 5°C / min to 1000°C, and keeping the temperature for 8 hours;

[0063] S3. Wash with acetic acid solution to obtain the electrocatalytic anode.

[0064] Experimental Example 1 The anode materials prepared in Examples 1-6 and Comparative Examples 1-2 were used to electrocatalytically oxidize simulated wastewater.

[0065] Prepare a bisphenol A aqueous solution with a COD of 198 mg / L, take 500 ml of the aqueous solution and put it in a 500 ml beaker, then put in the electrocatalytic anode prepared above with 0.01 m 2 The cathode uses a titanium plate, the plate spacing is 20 mm, the voltage is 5 V, the electrocatalytic oxidation is 0.5 h, and the COD value is tested using the national standard method. The results are shown in Table 1 below:

[0066]

[0067] In summary, the electrocatalytic oxidation method provided by the present invention is simple to operate, and when treating simulated low-COD organic wastewater, the treatment efficiency is above 80%, and can reach up to 84.8%.

[0068] Experimental Example 2 The ability of the electrocatalytic anode prepared in this scheme to treat industrial organic wastewater was investigated.

[0069] The electrocatalytic anode prepared in Example 1 was used for electrocatalytic oxidation treatment of organic wastewater with a COD concentration of 186 mg / L in a certain industrial park in Yueyang. During electrocatalytic oxidation, the distance between the anode plate and the cathode plate (titanium plate) was 20 mm, the voltage between the plates was 5 V, and the COD value detected by the national standard method was 32. The electrocatalytic anode material for treating organic wastewater prepared in this scheme had an efficiency of 82.8% in treating actual COD organic wastewater.

[0070] Experimental Example 3 The sensitivity of the electrocatalytic anode prepared in this scheme to the pH value of water was investigated.

[0071] Under the conditions of Experimental Example 2, the water body was adjusted to pH 2-12 with 1 mol / L sodium hydroxide solution or hydrochloric acid solution, and its treatment efficiency was tested. The results are shown in Table 2 below:

[0072]

[0073] The results show that the electrocatalytic anode prepared in Example 2 has a treatment efficiency of 80% or above in catalyzing COD organic wastewater in water bodies with different pH values, indicating that the electrocatalytic anode prepared in this scheme has low sensitivity to pH in the actual wastewater treatment process and is almost unaffected by pH, and is suitable for low COD wastewater with different pH values.

[0074] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and changes obtained without departing from the technical concept of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing an electrocatalytic anode material for treating organic wastewater, It is characterized in that The following steps are involved: S1, soaking the highly conductive substrate in an alkaline solution, drying it in an oven, and heating it to 300° C. in a tube furnace under an inert gas atmosphere to obtain a carrier material, which is then kept warm for later use; S2, soaking the carrier material prepared in S1 in an aqueous solution of a metal salt for adsorption loading, placing the adsorbed carrier material in an oven for drying, and then placing it in a tubular furnace under an inert gas atmosphere and heating it to 500-1000° C. for insulation; S3, washing the support material obtained in S2 with an acidic solution to obtain an electrocatalytic anode material; The highly conductive substrate in step S1 is selected from any one of activated carbon, graphite, and foamed metal; The alkaline solution in step S1 is selected from any one of sodium hydroxide solution, potassium hydroxide solution, sodium carbonate solution, and potassium phosphate solution; The metal salt in step S2 includes one or more of transition metal or noble metal chlorides, transition metal or noble metal sulfates, transition metal or noble metal nitrates, and transition metal or noble metal acetates.

2. The method for preparing an electrocatalytic anode material for treating organic wastewater according to claim 1, It is characterized in that The activated carbon is selected from any one of coconut shell activated carbon, wood activated carbon, fruit shell activated carbon, and coal activated carbon; the graphite is selected from any one of block graphite and flake graphite; the foam metal is selected from any one of foam nickel, foam copper, and foam titanium.

3. The method for preparing an electrocatalytic anode material for treating organic wastewater according to claim 1, It is characterized in that In the step S1, the drying temperature is 80°C, the drying time is 2 hours, the inert gas is selected from nitrogen or argon; the heating rate is 5°C / min; and the insulation time is 4 hours.

4. The method for preparing an electrocatalytic anode material for treating organic wastewater according to claim 1, It is characterized in that The transition metal includes one of iron, cobalt, nickel, copper and zinc, and the noble metal includes one of gold, silver, palladium and platinum.

5. The method for preparing an electrocatalytic anode material for treating organic wastewater according to claim 1, It is characterized in that In step S2, the mass of the metal salt is 5-20% of the carrier material, and the concentration of the aqueous solution of the metal salt is 2-10%.

6. The method for preparing an electrocatalytic anode material for treating organic wastewater according to claim 1, It is characterized in that The adsorption load time in step S2 is 4 hours; the drying temperature is 80-300°C, and the drying time is 2-4 hours; the inert gas is selected from nitrogen or argon; the heating rate is 5°C / min; and the insulation time is 4-8 hours.

7. The method for preparing an electrocatalytic anode material for treating organic wastewater according to claim 1, It is characterized in that The acidic solution in step S3 includes one of citric acid solution, oxalic acid solution, acetic acid solution, hydrochloric acid solution and hydrofluoric acid solution.

8. An electrocatalytic anode material for treating organic wastewater obtained by the preparation method according to any one of claims 1 to 7.

9. Use of the electrocatalytic anode material for treating organic wastewater prepared by the preparation method according to any one of claims 1 to 7 in treating low COD organic wastewater, It is characterized in that The application method is: putting the electrocatalytic anode material into 100-200 mg / L low COD organic wastewater, using a metal plate as the cathode, with a plate spacing of 2-50 mm, a voltage of 4-12 V, and electrocatalytic oxidation for 0.5 h.

10. The use according to claim 9, It is characterized in that The metal plate includes one of a titanium plate and an iron plate.