High damping manganese copper alloy and its cold spray additive manufacturing method and application

Through cold spray technology and subsequent treatment processes, the problem of insufficient damping performance of manganese-copper alloys is solved, the preparation of high-performance manganese-copper alloys is achieved, the process flow is simplified and the cost is reduced, and it is suitable for the rapid preparation of complex structural parts.

CN118527670BActive Publication Date: 2024-10-18GUANGDONG INST OF NEW MATERIALS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410969167.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-18
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing manganese-copper alloy damping performance cannot meet the high requirements of satellites, high-precision machine tools, ship propellers and other fields, and the preparation process is complex and costly.

Method used

Cold spray technology is used to deposit manganese-copper alloy powder on the surface of the substrate, and through solid solution treatment and aging treatment, the cold spray parameters are precisely controlled to improve the damping performance of the manganese-copper alloy and simplify the preparation process of complex structural parts.

Benefits of technology

The preparation of manganese-copper alloy with high damping performance is achieved, simplifying the process flow, reducing costs, and avoiding oxidation and stress cracking problems in thermal spraying and laser cladding repair processes, and the material properties are excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118527670B_ABST
    Figure CN118527670B_ABST
Patent Text Reader

Abstract

The present invention discloses a high damping manganese-copper alloy and its cold spray additive manufacturing method and application. The method comprises: depositing manganese-copper alloy powder on the surface of a substrate by cold spraying technology to form a manganese-copper alloy. During spraying, the carrier gas temperature is 300°C to 550°C, the carrier gas pressure is 3.0MPa to 6.0MPa, the spraying distance is 8 to 20mm, the spray gun movement rate is 80mm / min to 140mm / min, and the powder feeding rate is 20g / min to 30g / min; the manganese-copper alloy prepared by cold spraying is subjected to solution treatment and aging treatment in sequence. By adopting cold spraying technology to additively manufacture manganese-copper alloy, and accurately controlling the cold spraying parameters and combining the post-processing process (solid solution and aging), the high damping performance of the manganese-copper alloy is achieved, thereby realizing the preparation of a high-performance manganese-copper damping alloy with integrated structure and function.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of manganese-copper alloys, and in particular to a high-damping manganese-copper alloy and a cold spraying additive manufacturing method and application thereof. Background Art

[0002] Vibration and noise have a great impact on the working performance, reliability and stability of mechanical equipment, and even pose a threat to human life safety. Manganese copper alloy is a damping alloy with good vibration and noise reduction performance, which is widely used in civilian and military fields. Manganese copper alloy is a twin-crystal damping alloy. Due to the antiferromagnetic transformation of the γ phase in the alloy, a large number of lattice distortions are formed. The lattice distortion will induce the martensitic phase transformation and form a large number of martensitic twins. The manganese copper alloy has a high damping performance by relying on the interface movement between the parent phase and the unstable thermoelastic martensite and the movement of the martensitic twin interface to consume energy. However, the damping performance of the manganese copper alloy prepared by the existing preparation process can no longer meet the requirements of the material in the fields of satellites, high-precision machine tools or ship propellers.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The object of the present invention is to provide a high damping manganese-copper alloy and a cold spray additive manufacturing method and application thereof, so as to improve the above-mentioned technical problems.

[0005] The present invention is achieved in that:

[0006] In a first aspect, the present invention provides a method for cold spraying additive manufacturing of a high damping manganese-copper alloy, comprising:

[0007] A cold spraying technique is used to deposit manganese-copper alloy powder on the surface of a substrate to form a manganese-copper alloy. During spraying, the carrier gas temperature for loading the manganese-copper alloy powder is 300° C. to 550° C., the carrier gas pressure is 3.0 MPa to 6.0 MPa, the spraying distance is 8 to 20 mm, the spray gun movement rate is 80 mm / min to 140 mm / min, and the powder feeding rate is 20 g / min to 30 g / min.

[0008] The manganese-copper alloy prepared by cold spraying is subjected to solution treatment and aging treatment in sequence.

[0009] Optionally, during spraying, the carrier gas temperature for loading the manganese-copper alloy powder is 350°C~450°C, the carrier gas pressure is 4.0MPa~5.5MPa, the spraying distance is 8mm~12mm, the spray gun movement speed is 100mm / min~140mm / min, and the powder feeding rate is 20g / min~30g / min.

[0010] Optionally, the manganese-copper alloy powder is spherical in shape, and has a particle size of 15 μm to 55 μm.

[0011] Optionally, the particle size of the manganese-copper alloy powder is 20 μm to 55 μm.

[0012] Optionally, the chemical composition of the manganese-copper alloy powder is, by weight percentage, Cu 10-30%, Ni 2-10%, Fe 1-5%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the remainder is Mn element and other inevitable impurities.

[0013] Optionally, the chemical composition of the manganese-copper alloy powder is, by weight percentage, Cu 15-26%, Ni 2-7%, Fe 1-5%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the remainder is Mn element and other inevitable impurities.

[0014] Optionally, the solution treatment includes: keeping the temperature at 800°C to 950°C for 0.5h to 2h, and cooling to room temperature;

[0015] Optionally, the aging treatment includes: keeping the temperature at 360° C. to 550° C. for 1 h to 100 h, and cooling to room temperature.

[0016] Optionally, the substrate may be grit blasted prior to cold spraying to remove scale and stains.

[0017] In a second aspect, the present invention also provides a high damping manganese-copper alloy, which is prepared by the above-mentioned method for cold spraying additive manufacturing of high damping manganese-copper alloy.

[0018] In a third aspect, the present invention also provides the use of the above-mentioned high damping manganese-copper alloy in the preparation of satellites, rail transportation, high-precision machine tools or ship propellers.

[0019] The present invention has the following beneficial effects: by using cold spraying technology to additively manufacture manganese-copper alloys, and accurately controlling the cold spraying parameters and combining post-treatment processes (solid solution and aging), the high damping performance of the manganese-copper alloy is achieved, thereby realizing the preparation of high-performance manganese-copper damping alloys with integrated structural functions. In addition, the additive manufacturing method of manganese-copper alloys prepared by cold spraying technology is suitable for the rapid preparation of complex damping structural parts, which can effectively simplify the preparation process of complex damping structural parts and reduce costs. Moreover, compared with thermal spraying and laser cladding repair processes, the manganese-copper alloy prepared by cold spray additive manufacturing has a fast forming speed and finer grains, which can avoid problems such as oxidation and stress cracking, and has excellent comprehensive performance such as material damping performance and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0021] Figure 1 This is a SEM image of the manganese-copper alloy powder used in Example 1 of the present invention;

[0022] Figure 2 The CT result diagram of the pore morphology and three-dimensional spatial distribution of the manganese-copper alloy product obtained in Example 1 of the present invention;

[0023] Figure 3 The amplitude damping spectra of the manganese-copper alloy products prepared in Examples 1 to 10 of the present invention and Comparative Examples 1 to 2 at room temperature are shown;

[0024] Figure 4 This is a SEM image of each manganese-copper alloy product prepared in Comparative Example 3 of the present invention;

[0025] Figure 5 This is the amplitude damping spectrum of each manganese-copper alloy product prepared in Comparative Example 3 of the present invention at room temperature. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0027] The following is a detailed description of a high damping manganese-copper alloy provided by the present invention and its cold spray additive manufacturing method and application.

[0028] Some embodiments of the present invention provide a method for cold spraying additive manufacturing of high damping manganese-copper alloy, which comprises: depositing manganese-copper alloy powder on the surface of a substrate using cold spraying technology to form a manganese-copper alloy. During spraying, the carrier gas temperature for loading the manganese-copper alloy powder is 300°C~550°C, the carrier gas pressure is 3.0MPa~6.0MPa, the spraying distance is 8~20mm, the spray gun movement rate is 80mm / min~140mm / min, and the powder feeding rate is 20g / min~30g / min; the manganese-copper alloy prepared by cold spraying is subjected to solution treatment and aging treatment in sequence.

[0029] The inventor creatively adopted the cold spraying technology for additive manufacturing of manganese-copper alloy. Cold spraying is a deposition technology that uses supersonic airflow to cause completely solid powder particles to collide with the matrix, and the plastic deformation generated by the collision causes the powder-matrix and powder-powder to combine. The formation of cold spray deposits mainly depends on the kinetic energy of the particles before the collision rather than the thermal energy, so the cold spray particles remain solid during the entire deposition process. Since the powder does not melt during the cold spraying process, the bonding between the particles is mainly achieved through mechanical interlocking and local metallurgical bonding at the interface between the particles. Since cold spraying has the characteristics of low-temperature molding, the material will not oxidize, which has obvious advantages over thermal spraying technology and high-energy ion beam additive manufacturing technology. At the same time, the low heat input of cold spraying technology can effectively avoid the growth of material grains, phase changes and the generation of thermal stress, which is an excellent molding technology for heat-sensitive materials and easily oxidized materials.

[0030] The above embodiments of the present invention achieve high damping performance of manganese-copper alloy by precisely controlling cold spraying parameters and combining post-treatment processes (solid solution and aging), thereby realizing the preparation of high-performance manganese-copper damping alloy with integrated structure and function. Among them, the alloy elements are fully dissolved in the matrix through solid solution treatment to form a supersaturated solid solution, which provides conditions for subsequent aging treatment, and can eliminate the microsegregation and residual stress that may be generated during the cold spraying process to a certain extent, and improve the uniformity of the material's organizational structure; and the supersaturated austenite of the manganese-copper alloy undergoes spinodal decomposition during the aging process, and a manganese-rich matrix and copper-rich nanoparticles are formed during the spinodal decomposition process, and the formation of the manganese-rich matrix enhances the damping performance of the manganese-copper alloy.

[0031] It should be noted that the parameters of cold spraying are particularly critical to the damping performance of manganese-copper alloy, especially the carrier gas temperature. If the temperature is too low, the manganese-copper alloy powder will have poor deformability and poor bonding between the powders; if the temperature is too high, pure manganese phase will precipitate, inhibiting the movement of the martensitic twin interface in the manganese-rich matrix, resulting in poor damping performance. The carrier gas pressure and spraying distance will also affect the effect of cold spraying to a certain extent. For example, too low a spraying pressure or too long a spraying distance may cause the manganese-copper alloy powder to fail to reach the optimal kinetic energy and cause poor bonding performance. Too high a pressure or too close a spraying distance may result in a high dislocation density.

[0032] Specifically, during spraying, the carrier gas temperature for loading the manganese-copper alloy powder is 300°C to 550°C. Exemplarily, it can be selected as 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C or 550°C, etc., or a temperature between any two of the above temperatures. The carrier gas pressure is 3.0 MPa to 6.0 MPa. For example, it can be selected as 3.0 MPa, 3.1 MPa, 3.2 MPa, 3.3 MPa, 3.4 MPa, 3.5 MPa, 3.6 MPa, 3.7 MPa, 3.8 MPa, 3.9 MPa, 4.0 MPa, 4.1 MPa, 4.2 MPa, 4.3 MPa, 4.4 MPa, 4.5 MPa, 4.6 MPa, 4.7 MPa, 4.8 MPa, 4.9 MPa, 5 MPa, 5.1 MPa, 5.2 MPa, 5.3 MPa, 5.4 MPa, 5.5 MPa, 5.6 MPa, 5.7 MPa, 5.8 MPa, 5.9 MPa or 6.0 MPa, or a pressure between any two of the above pressures. The spraying distance is 8-20 mm, and for example, the spraying distance can be selected as 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm or 20 mm, etc. The movement rate of the spray gun is 80 mm / min-140 mm / min, and for example, it can be selected as 80 mm / min, 90 mm / min, 100 mm / min, 110 mm / min, 120 mm / min, 130 mm / min or 140 mm / min, etc. The powder feeding rate is 20 g / min-30 g / min, and for example, it can be selected as 20 g / min, 21 g / min, 22 g / min, 23 g / min, 24 g / min, 25 g / min, 26 g / min, 27 g / min, 28 g / min, 29 g / min or 30 g / min, etc.

[0033] Furthermore, in order to achieve better damping performance, the above cold spraying process parameters were optimized. In some embodiments, during spraying, the carrier gas temperature used to load the manganese-copper alloy powder is 350°C~450°C, the carrier gas pressure is 4.0MPa~5.5MPa, the spraying distance is 8mm~12mm, the spray gun moving speed is 100mm / min~140mm / min, and the powder feeding rate is 20g / min~30g / min.

[0034] For reference, in some embodiments, the shape of the above-mentioned manganese-copper alloy powder is spherical and the particle size is 15μm~55μm. In the method for preparing manganese-copper alloy by cold spraying additive in the embodiment of the present invention, the particle size of the manganese-copper alloy powder used for cold spraying has an important influence on the damping performance of the manganese-copper alloy finally obtained. In theory, the larger the particle size of the manganese-copper alloy powder, the better the damping performance. However, if the manganese-copper alloy powder is too large, it will lead to a small degree of deformation and poor bonding, thereby reducing both the damping performance and the mechanical properties. Therefore, it is necessary to control the particle size of the manganese-copper alloy powder within a certain range to achieve a better cold spraying effect and greatly improve the damping performance. Exemplarily, the particle size of the manganese-copper alloy powder can be selected as 20μm~55μm or 30μm~55μm or 30μm~45μm, etc.

[0035] Furthermore, in order to achieve the required formation of a manganese-rich matrix and copper-rich nanoparticles in the manganese-copper alloy and the number of martensitic twins, it is necessary to design the chemical composition of the manganese-copper alloy so that it can achieve the required damping performance. Exemplarily, by weight percentage, the chemical composition of the manganese-copper alloy powder is: Cu 10-30%, Ni 2-10%, Fe 1-5%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the balance is Mn element and other unavoidable impurities. Or, by weight percentage, the chemical composition of the manganese-copper alloy powder is: Cu 15-26%, Ni 2-7%, Fe 1-5%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the balance is Mn element and other unavoidable impurities.

[0036] In some embodiments, the carrier gas used for cold spraying can be helium, nitrogen, argon, etc.

[0037] In some embodiments, the substrate in the above embodiments may be selected from sandblasted steel, copper alloy, manganese copper alloy, etc. That is, before cold spraying, the substrate may be sandblasted to remove oxide scale and stains.

[0038] In some embodiments, the nozzle used for cold spraying is a SiC Laval nozzle.

[0039] For reference, the solution treatment includes: keeping the temperature at 800°C to 950°C for 0.5h to 2h, and cooling to room temperature. For example, the solution treatment temperature can be selected as 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C or 950°C, etc., and the holding time is 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h or 2.0h, etc. In some embodiments, the solution treatment is performed in a heating furnace, and after the sample is taken out, it is quickly placed in water and cooled to room temperature to obtain a supersaturated γMn-Cu solid solution.

[0040] For reference, the aging treatment includes: keeping the temperature at 360°C to 550°C for 1h to 100h, and cooling to room temperature. For example, the aging treatment temperature can be selected as 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C or 550°C. In some embodiments, the aging treatment is also carried out in a heating furnace, and the sample is taken out and placed in the air to cool to room temperature.

[0041] Some embodiments of the present invention also provide a high damping manganese-copper alloy, which is prepared by the above-mentioned method for cold spraying additive manufacturing of high damping manganese-copper alloy. In some embodiments, the porosity of the high damping manganese-copper alloy is less than 2%.

[0042] Some embodiments of the present invention also provide the use of the above-mentioned high-damping manganese-copper alloy in the preparation of satellites, rail transportation, high-precision machine tools or ship propellers.

[0043] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0044] Example 1

[0045] This embodiment provides a method for cold spraying additive manufacturing of high damping manganese-copper alloy, which specifically includes the following steps:

[0046] The copper plate is first sandblasted to remove the oxide scale and stains on the cold sprayed surface of the copper plate and used as a substrate before cold spraying.

[0047] The powder with a particle size of 30~45μm was used (SEM image as shown in Figure 1As shown in the figure, cold spraying additive manufacturing of manganese-copper alloy was carried out. The spraying parameters were: the working carrier gas was helium, the carrier gas temperature was 450°C, the carrier gas pressure was 4.5MPa, the spraying distance was 10mm, the spray gun moving speed was 120mm / min, the powder feeding speed was 25g / min, and the coating thickness was 6mm.

[0048] The manganese-copper alloy prepared by cold spraying was placed in a heat treatment furnace, kept at 900°C for 1 hour, and water-cooled. Then, the quenched manganese-copper alloy was placed in a heat treatment furnace, aged at 475°C for 12 hours, and air-cooled to room temperature.

[0049] The chemical composition of the manganese-copper alloy powder used for cold spray additive manufacturing technology is as follows by weight percentage: Cu content 22%, Ni content 5%, Fe content 2%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the balance is Mn element and other unavoidable impurities.

[0050] Example 2

[0051] This embodiment provides a method for cold spraying additive manufacturing of high damping manganese-copper alloy, which specifically includes the following steps:

[0052] The copper plate is first sandblasted to remove the oxide scale and stains on the cold sprayed surface of the copper plate and used as a substrate before cold spraying.

[0053] Powder with a particle size of 40~55μm was used for cold spray additive manufacturing of manganese-copper alloy. The spraying parameters were: the working carrier gas was helium, the carrier gas temperature was 400℃, the carrier gas pressure was 4.0MPa, the spraying distance was 10mm, the spray gun moving speed was 120mm / min, the powder feeding rate was 25g / min, and the coating thickness was 6mm.

[0054] The manganese-copper alloy prepared by cold spraying was placed in a heat treatment furnace, kept at 880°C for 1.5 hours, and water-cooled. The quenched manganese-copper alloy was then placed in a heat treatment furnace, aged at 450°C for 18 hours, and air-cooled to room temperature.

[0055] Measured by weight percentage, the chemical composition of the manganese-copper alloy powder used for cold spray additive manufacturing technology is: Cu content 26%, Ni content 7%, Fe content 5%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the balance is Mn element and other unavoidable impurities.

[0056] Example 3

[0057] This embodiment provides a method for cold spraying additive manufacturing of high damping manganese-copper alloy, which specifically includes the following steps:

[0058] The copper plate is first sandblasted to remove the oxide scale and stains on the cold sprayed surface of the copper plate and used as a substrate before cold spraying.

[0059] Powder with a particle size of 20~35μm was used for cold spray additive manufacturing of manganese-copper alloy. The spraying parameters were: the working carrier gas was helium, the carrier gas temperature was 350℃, the carrier gas pressure was 5.5MPa, the spraying distance was 10mm, the spray gun moving speed was 120mm / min, the powder feeding rate was 25g / min, and the coating thickness was 6mm.

[0060] The manganese-copper alloy prepared by cold spraying was placed in a heat treatment furnace, kept at 850°C for 2 hours, and water-cooled. The quenched manganese-copper alloy was then placed in a heat treatment furnace, aged at 440°C for 30 hours, and air-cooled to room temperature.

[0061] The chemical composition of the manganese-copper alloy powder used for cold spray additive manufacturing technology is as follows by weight percentage: Cu content 15%, Ni content 2%, Fe content 1%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the balance is Mn element and other unavoidable impurities.

[0062] Example 4

[0063] The difference from Example 1 is that the carrier gas temperature of this example is 550° C., and the rest of the contents are consistent with Example 1.

[0064] Example 5

[0065] The only difference from Example 1 is that in this embodiment, the manganese-copper alloy powder manufactured by cold spraying additive manufacturing has a particle size of less than 15 μm.

[0066] Example 6

[0067] The only difference from Example 1 is that in this embodiment, the manganese-copper alloy powder manufactured by cold spraying additive manufacturing has a particle size of 50-65 μm.

[0068] Example 7

[0069] The only difference from Example 1 is that in this embodiment, the manganese-copper alloy powder manufactured by cold spraying additive manufacturing has a chemical composition, by weight percentage, of Cu 10%, Ni 1%, Fe 1%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the remainder is Mn element and other inevitable impurities.

[0070] Example 8

[0071] The only difference from Example 1 is that in this comparative example, the manganese-copper alloy powder manufactured by cold spraying additive manufacturing has a chemical composition, by weight percentage, of Cu 30%, Ni 10%, Fe 10%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the remainder is Mn element and other inevitable impurities.

[0072] Comparative Example 1

[0073] The only difference from Example 1 is that in this comparative example, the manganese-copper alloy manufactured by cold spraying is not subjected to any heat treatment (solution treatment and aging treatment).

[0074] Comparative Example 2

[0075] The only difference from Example 1 is that in this comparative example, the manganese-copper alloy prepared by cold spraying is placed in a heat treatment furnace, kept at 900° C. for 1 hour, and water-cooled without further aging treatment.

[0076] Comparative Example 3

[0077] The only difference between this comparative example and comparative example 1 is that the cold spray additive manufacturing uses manganese-copper alloy powders with a particle size of less than 25 μm and a particle size of 15-53 μm for additive manufacturing at carrier gas temperatures of 300°C, 400°C and 500°C, respectively.

[0078] Experimental example

[0079] The pore morphology and three-dimensional spatial distribution of the manganese-copper alloy obtained in Example 1 were analyzed, and the CT results were as follows: Figure 2 As shown by Figure 2 The results show that the density of the manganese-copper alloy can reach 98.7%.

[0080] The manganese-copper alloys prepared in Examples 1-8 and Comparative Examples 1-2 were tested for damping performance. The damping performance test of the samples was performed using a dynamic thermal mechanical analyzer (DMA Q850) in a single cantilever mode. The sample size was 32×4×1 mm 3 , the vibration frequency f = 1 Hz, the vibration strain is 1×10 -5 -1×10 -3 The experimental results are as follows Figure 3 shown.

[0081] The results of scanning electron microscopy observation of the manganese-copper alloys obtained in Comparative Example 3 are as follows: Figure 4 As shown. Figure 4It can be seen that as the temperature increases, the bonding quality of the particles in the sample improves. In the sample with a lower cold spray temperature, due to the lower impact velocity of the powder, cracks appear at the bonding point between the powders and holes are generated due to uneven deformation of the powders. As the temperature increases, such cracks and holes are improved. The manganese-copper alloy prepared in Comparative Example 3 was tested for damping properties. The results are as follows: Figure 5 As shown. Figure 5 It can be seen from the amplitude spectrum that the damping performance gradually increases with the increase of strain amplitude. In the original state of cold spraying, the damping performance of coarse powder is generally higher than that of fine powder, and the damping performance is higher when the cold spraying temperature is 400℃, and lower when it is 500℃. The reason for this phenomenon is that the deformation of fine powder after cold spraying is more serious, resulting in a decrease in the damping performance of the material.

[0082] In summary, the embodiment of the present invention adopts cold spraying technology to prepare high damping manganese-copper alloy. By accurately controlling the process parameters of cold spraying, the bonding and recrystallization between powder particles in the deposition process are promoted, and then combined with solution treatment and aging treatment, the high damping performance of manganese-copper alloy is achieved, thereby realizing the preparation of high-performance manganese-copper damping alloy with integrated structure and function. In addition, the additive manufacturing method of manganese-copper alloy prepared by cold spraying technology is suitable for the rapid preparation of complex damping structural parts, which can effectively simplify the preparation process of complex damping structural parts and reduce costs. Moreover, compared with thermal spraying and laser cladding repair processes, the manganese-copper alloy prepared by cold spraying additive manufacturing has a fast forming speed and finer grains, which can avoid problems such as oxidation and stress cracking, and the material has excellent comprehensive performance such as damping performance and mechanical properties.

[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for cold spraying additive manufacturing of high damping manganese copper alloy, characterized in that: It includes: A cold spraying technique is used to deposit manganese-copper alloy powder on the surface of a substrate to form a manganese-copper alloy. During spraying, the carrier gas temperature for loading the manganese-copper alloy powder is 300° C. to 550° C., the carrier gas pressure is 3.0 MPa to 6.0 MPa, the spraying distance is 8 to 20 mm, the spray gun movement rate is 80 mm / min to 140 mm / min, and the powder feeding rate is 20 g / min to 30 g / min. The particle size of the manganese-copper alloy powder is 20 μm to 55 μm; The chemical composition of the manganese-copper alloy powder is: Cu 10-30%, Ni 2-10%, Fe 1-5%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the balance is Mn element and other inevitable impurities; The manganese-copper alloy prepared by cold spraying is subjected to solution treatment and aging treatment in sequence; The solution treatment comprises: keeping the temperature at 800°C to 950°C for 0.5h to 2h, and cooling to room temperature; The aging treatment comprises: keeping the temperature at 360° C. to 550° C. for 1 h to 100 h, and cooling to room temperature.

2. The method according to claim 1, characterized in that During spraying, the carrier gas temperature for loading the manganese-copper alloy powder is 350° C. to 450° C., the carrier gas pressure is 4.0 MPa to 5.5 MPa, the spraying distance is 8 mm to 12 mm, the spray gun moving speed is 100 mm / min to 140 mm / min, and the powder feeding rate is 20 g / min to 30 g / min.

3. The method according to claim 1, characterized in that Calculated by weight percentage, the chemical composition of the manganese-copper alloy powder is: Cu 15-26%, Ni 2-7%, Fe 1-5%, O≤0.2%, S≤0.01%, C≤0.01%, N≤0.005%, and the remainder is Mn element and other inevitable impurities.

4. The method according to any one of claims 1 to 3, characterized in that Prior to cold spraying, the substrate is grit blasted to remove scale and stains.

5. A high damping manganese-copper alloy, characterized in that: It is prepared by the method described in any one of claims 1 to 4.

6. Use of the high damping manganese-copper alloy as claimed in claim 5 in the preparation of satellites, rail transportation, high-precision machine tools or ship propellers.

Citation Information

Patent Citations

  • Manganese-copper damping alloy powder for SLM process and preparation method thereof

    CN111057922A

  • Preparation method for CuW / CuCr integrated contact

    CN112658243A

  • Resistor and circuit substrate

    US20210225562A1