Compressed glaze based on cordierite powder, preparation method of compressed glaze slurry and insulator

By introducing specific proportions of potassium feldspar, quartz powder, wollastonite, Guangxi white mud, elutriated faku soil, cordierite powder, barium carbonate and manganese dioxide into the compressed glaze, a synergistic glaze is formed. It solves the problem of imbalance in viscosity, glazing strength, melting temperature and flow value, reduces the expansion coefficient, and improves the product's operability and surface quality.

CN118529933BActive Publication Date: 2024-10-22超创数能科技有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995065.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-22
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

During the preparation and application process of compressed glaze, the existing technology is difficult to balance the viscosity, glaze strength, melting temperature and flow value, resulting in uncontrolled glazing operation, low product surface quality, high expansion coefficient, and prone to thermal expansion. Mismatch and cracks.

Method used

By introducing 14% to 18% potash feldspar, 6% to 10% quartz powder, 10% to 14% wollastonite, 3% to 7% Guangxi white mud, and 7% to 11% elutriation method Library soil, 43% ~ 47% Cordierite powder, 1% to 5% barium carbonate, and 1% to 3% manganese dioxide form a synergistic compressed glaze to ensure that the viscosity, glaze strength, melting temperature and flow value are balanced, and reduce expansion coefficient.

Benefits of technology

It achieves controllability of glazing operation, improves product surface quality, enhances mechanical strength and durability, reduces thermal expansion stress and cracks, and meets high-standard application requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118529933B_ABST
    Figure CN118529933B_ABST
Patent Text Reader

Abstract

The present application provides a compressed glaze based on cordierite powder, a method for preparing a compressed glaze slurry, and an insulator. The compressed glaze based on cordierite powder provided in the present application comprises the following chemical components: SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O, TiO2, BaO, and MnO2; in terms of weight percentage, the chemical components in the compressed glaze are introduced by 14% to 18% of potassium feldspar, 6% to 10% of quartz powder, 10% to 14% of wollastonite, 3% to 7% of Guangxi white mud, 7% to 11% of washed Faku soil, 43% to 47% of cordierite powder, 1% to 5% of barium carbonate, and 1% to 3% of manganese dioxide; the synergistic effect of potassium feldspar, wollastonite, and cordierite powder in the compressed glaze leads to a balance in viscosity, glazing strength, melting temperature, and flow value of the compressed glaze, and reduces the expansion coefficient. The compressed glaze based on cordierite powder, the preparation method of compressed glaze slurry and the insulator provided in the present application can ensure that the glaze exhibits excellent operating performance during the glazing and firing processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of compressed glazes, and in particular to a compressed glaze based on cordierite powder, a method for preparing a compressed glaze slurry, and an insulator. Background Art

[0002] Glaze is a thin layer of glass attached to the surface of ceramic body. It is made of mineral raw materials in a certain proportion, ground into glaze slurry, applied to the surface of the body, and calcined at a certain temperature. After the glaze is attached to the body and calcined at a high temperature, it can improve the mechanical strength of the porcelain due to its compressive effect on the porcelain.

[0003] For the straight-head structure products commonly used in the current industry, the main stress position is concentrated on the head of the product. Therefore, compression glaze will be applied to the head of the product to improve the mechanical strength of the product and stabilize the product strength.

[0004] In the preparation and application of compressed glazes, in order to ensure the controllability of the glazing operation and improve the surface quality of the product, it is necessary to ensure a balance between the viscosity, glazing strength, melting temperature and flow value of the compressed glaze. Summary of the invention

[0005] In view of this, the present application provides a compressed glaze based on cordierite powder, a method for preparing compressed glaze slurry and an insulator, so as to reduce the expansion coefficient of the compressed glaze while ensuring that the viscosity, glazing strength, melting temperature and flow value of the compressed glaze are balanced, so as to ensure the controllability of the glazing operation and improve the surface quality of the product.

[0006] Specifically, the present application is implemented through the following technical solutions:

[0007] In a first aspect, the present application provides a compressed glaze based on cordierite powder, the compressed glaze comprising the following chemical components: SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O, TiO2, BaO, MnO2;

[0008] According to weight percentage, the chemical components in the compressed glaze are introduced by 14% to 18% potassium feldspar, 6% to 10% quartz powder, 10% to 14% wollastonite, 3% to 7% Guangxi white mud, 7% to 11% washed Faku clay, 43% to 47% cordierite powder, 1% to 5% barium carbonate, and 1% to 3% manganese dioxide;

[0009] The synergistic effect of potassium feldspar, wollastonite and cordierite powder in the compressed glaze leads to a balance in viscosity, glazing strength, melting temperature and flow value of the compressed glaze, and reduces the expansion coefficient.

[0010] The second aspect of the present application provides a method for preparing a compressed glaze slurry, wherein the method uses any one of the compressed glaze materials provided in the first aspect of the present application to prepare a compressed glaze slurry; the method comprises:

[0011] Hydration treatment is performed on the potassium feldspar, quartz powder, wollastonite, cordierite powder, barium carbonate and manganese dioxide in the compressed glaze to obtain a first mixed slurry;

[0012] Using a ball mill to perform a ball milling operation on the first mixed slurry, Guangxi white mud and washed Faku soil in the compressed glaze to obtain a second mixed slurry;

[0013] filtering the second mixed slurry to obtain filtered slurry;

[0014] The filtered slurry is subjected to iron removal treatment to obtain the compressed glaze slurry.

[0015] A third aspect of the present application provides an insulator, the head of which is glazed based on the compressed glaze slurry provided in the second aspect of the present application.

[0016] The compressed glaze provided by the present application introduces SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O, TiO2, BaO, and MnO2 into the compressed glaze by utilizing 14% to 18% of potassium feldspar, 6% to 10% of quartz powder, 10% to 14% of wollastonite, 3% to 7% of Guangxi white mud, 7% to 11% of washed Faku soil, 43% to 47% of cordierite powder, 1% to 5% of barium carbonate, and 1% to 3% of manganese dioxide. In this way, firstly, potassium feldspar acts as a flux to reduce the melting temperature and viscosity of the glaze, while wollastonite and cordierite powder can provide a certain balance of structure and viscosity, so that the glaze has an appropriate viscosity when glazing, and is easy to control and apply. Covering; secondly, the glass phase formed by potassium feldspar during the firing process can enhance the strength of the glaze layer, while the structural support provided by wollastonite and cordierite powder can improve the mechanical strength of the glaze layer, so that the glaze has a higher glazing strength and avoids cracking and peeling; thirdly, while potassium feldspar reduces the melting temperature, wollastonite and cordierite powder ensure that the glaze melts and flows within the appropriate temperature range, and will not cause excessive flow due to too low melting temperature, or difficult to melt due to too high melting temperature; fourthly, potassium feldspar can improve fluidity and ensure that the glaze can be evenly covered in the molten state, while wollastonite and cordierite powder can adjust this fluidity so that the glaze will not flow excessively during the melting process, thereby forming a uniform and appropriately thick glaze layer. That is, through the synergistic effect of potassium feldspar, wollastonite and cordierite powder, the viscosity, glazing strength, melting temperature and flow value of the compressed glaze can be balanced.

[0017] In addition, both wollastonite and cordierite powder have low expansion coefficients. By introducing wollastonite and cordierite powder, the overall expansion coefficient of the glaze is significantly reduced, reducing the stress and cracks caused by thermal expansion mismatch during heat treatment.

[0018] Furthermore, when the viscosity, glazing strength, melting temperature and flow value are balanced, it can not only ensure that the glaze exhibits excellent operating performance during glazing and firing, but also ensure that the surface quality of the final product is high, so that it has good mechanical strength, smoothness and durability, thereby meeting the high standards required in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a flow chart of Example 1 of the method for preparing compressed glaze slurry provided in the present application. DETAILED DESCRIPTION

[0020] Here, exemplary embodiments are described in detail, and examples thereof are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The implementations described in the following exemplary embodiments do not represent all implementations consistent with the present application.

[0021] The terms used in this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application are also intended to include plural forms, unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used in this article refers to and includes any or all possible combinations of one or more associated listed items.

[0022] It should be understood that although the terms first, second, third, etc. may be used in the present application to describe various information, these information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present application, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Depending on the context, the word "if" as used herein may be interpreted as "at the time of" or "when" or "in response to determining".

[0023] Specific embodiments are given below to introduce the technical solution of the present application in detail.

[0024] Specifically, the present application provides a compressed glaze based on cordierite powder, wherein the compressed glaze comprises the following chemical components: SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O, TiO2, BaO, MnO2;

[0025] The chemical components in the compressed glaze are introduced by 14% to 18% potassium feldspar, 6% to 10% quartz powder, 10% to 14% wollastonite, 3% to 7% Guangxi white mud, 7% to 11% washed Faku clay, 43% to 47% cordierite powder, 1% to 5% barium carbonate, and 1% to 3% manganese dioxide;

[0026] The synergistic effect of potassium feldspar, wollastonite and cordierite powder in the compressed glaze leads to a balance in viscosity, glazing strength, melting temperature and flow value of the compressed glaze, and reduces the expansion coefficient.

[0027] It should be noted that the viscosity of compressed glaze refers to the viscosity required in the process of preparing and applying compressed glaze. Generally speaking, the viscosity of compressed glaze should be low enough to be smoothly coated on the surface of the substrate and to fill fine pores and surface unevenness to ensure the formation of a uniform and dense glaze layer. On the other hand, the viscosity should not be too low, otherwise it may cause the glaze layer to flow or produce vertical flow after coating, affecting the uniformity of coating and the forming effect.

[0028] The glazing strength of compression glaze refers to the tensile strength range of the glaze layer formed after being applied to the surface of the substrate, which reflects the resistance of the glaze layer under bending stress.

[0029] The melting temperature range of compressed glaze refers to the temperature range in which the compressed glaze begins to soften and form a liquid during the heating or sintering process. This range usually refers to the interval between the temperature at which the compressed glaze begins to soften and the temperature at which it is completely melted.

[0030] The flow value of compressed glaze refers to the ability of the glaze to flow and spread when it forms a liquid on the surface during sintering or heating. It is expressed as the distance or area that the glaze flows at a specific temperature. This value is usually a quantitative indicator used to describe the flow properties of the glaze in a molten state.

[0031] The expansion coefficient of a compressed glaze refers to the relationship between the volume expansion of the glaze and the temperature change during sintering or heating.

[0032] The following describes the test methods for each performance parameter:

[0033] 1. Expansion coefficient

[0034] Specifically, the expansion coefficient of the compressed glaze is measured by the following method:

[0035] (1) Prepare compressed glaze samples. First, mix the glaze and diluent in a certain ratio until a uniform liquid glaze is formed. Select a suitable substrate as the carrier of the compressed glaze. Common substrates include ceramic sheets, tiles, metal sheets, etc. The prepared glaze is evenly coated on the surface of the substrate, and then the substrate coated with the glaze is dried. The dried substrate is placed in a kiln for firing, and finally the fired sample is cooled and corrected;

[0036] (2) Mark reference points on the sample to measure length changes and record the sample's initial length, width, thickness and other data;

[0037] (3) Fix the sample on the thermal expansion instrument, determine the parameters of the thermal expansion instrument such as the heating rate and target temperature according to the test requirements, and record the length, width, thickness and other data of the sample during the test;

[0038] (4) Calculate the coefficient of thermal expansion based on the length change and temperature change of the sample during the test.

[0039] 2. Viscosity

[0040] Optionally, in a possible implementation manner, the viscosity of the compressed glaze is measured by a viscosity testing method specified in GBT22235-2008 standard.

[0041] Specifically, the viscosity test method specified in the GBT 22235-2008 "Test Methods for Rheological Properties of Ceramic Glazes" standard is as follows:

[0042] (1) Prepare the sample. Heat the glaze sample in a hot water bath to the test temperature.

[0043] Specifically, when conducting a viscosity test, the test temperature usually varies depending on the type of glaze and the application scenario. Typically, the temperature range of the viscosity test may be between 800°C and 1300°C.

[0044] (2) Adjust the viscometer and select the appropriate rotor and speed according to the test temperature and the expected viscosity of the glaze.

[0045] (3) To measure the viscosity, pour the heated glaze sample into a sampling container, place the viscometer in the center of the glaze, and start measuring the viscosity.

[0046] (4) Record the viscometer data within the specified time.

[0047] 3. Melting temperature

[0048] In the present application, the melting temperature refers to the temperature between when the cylindrical sample prepared based on the compressed glaze begins to melt (the cylindrical sample becomes a hemispherical shape) and when it begins to flow (the cylindrical sample becomes a flat shape) under the action of temperature.

[0049] Specifically, the melting start temperature is the temperature at which a cylindrical sample changes into a hemispherical shape, and the flowing start temperature is the temperature at which a cylindrical sample flows and becomes flat.

[0050] The melting temperature of glaze is crucial to the firing quality of electric porcelain. If the melting temperature is too low, the glaze will cover the body before it is sintered, completely sealing the open pores, which may easily cause glaze bubbles on the porcelain after the kiln. If the melting temperature is too high, the body will not be well infiltrated, resulting in defects such as rough glaze surface and poor gloss.

[0051] The melting temperature range is determined by firing a number of Φ5×5mm cylindrical samples (usually 7 to 9) made of glaze at different temperatures with an interval of 20°C at high temperature, and observing the changes in the appearance of the samples after firing.

[0052] The significance of glaze changes at various temperature points:

[0053] 1. Softening temperature: The edges and corners of the cylindrical specimen begin to become slightly rounded;

[0054] 2. Beginning melting temperature: the cylindrical sample changes into a hemispherical shape;

[0055] 3. Beginning flow temperature: The sample flows and becomes flat;

[0056] 4. Softening temperature range: the temperature range between the beginning of softening and the beginning of melting;

[0057] 5. Melting temperature range: the temperature range between the beginning of melting and the beginning of flow.

[0058] It should be noted that the instruments and apparatus required to determine the melting temperature range of compressed glazes include:

[0059] (1) Metal mold: Φ5×30mm;

[0060] (2) Sieve; mesh size 0.15 mm (100 mesh standard sieve);

[0061] (3) Rectangular dry mud block: 40×10×8mm;

[0062] (4) Mallet, paper cutter, CMC gel;

[0063] (5) High temperature electric furnace: the maximum temperature is not less than 1350℃.

[0064] The specific test method for the melting temperature range is introduced below:

[0065] Specifically, in a possible implementation, the melting temperature range of the compressed glaze is measured by the following method:

[0066] (1) Based on the compressed glaze, a preset number of cylindrical samples of a preset size are prepared according to a high temperature fluidity test sample preparation method.

[0067] Specifically, the preparation of the cylindrical sample is to add CMC gel to the dry glaze powder until the powder is slightly moist. Put the evenly mixed powder into a metal mold with a size of Φ5×30mm and pound it into a Φ5×5mm cylinder. If the sample is too high, sandpaper or a paper cutter can be used to trim the sample height to 5mm. The upper and lower surfaces of the cylindrical sample are required to be flat and have clear edges and corners. Dry the sample to make a cylindrical sample. It should be noted that the preset number of cylindrical samples is about 7 to 9.

[0068] (2) Smoothing the bottom surface of the cylindrical sample, and gluing the cylindrical sample to the rectangular mud block through CMC gel in a manner that the bottom surface of the cylindrical sample is opposite to the rectangular mud block, to obtain a test glaze column; wherein each test glaze column is marked with a corresponding preset firing temperature.

[0069] (3) For each test glaze column, the test glaze column is fired in an electric furnace at its corresponding preset firing temperature to obtain a fired sample; wherein each test glaze column is kept warm for a preset time after reaching the preset firing temperature.

[0070] Specifically, in a possible implementation, the insulation time is 15 minutes, and the maximum temperature of the electric furnace is not less than 1350°C.

[0071] (4) placing the fired sample into an annealing furnace for annealing to obtain an annealed sample.

[0072] Among them, annealing is to eliminate the residual stress inside the sample and improve the quality and stability of the sample.

[0073] (5) Cool the annealed sample to room temperature to obtain a final sample.

[0074] (6) Determining a melting temperature range of the compressed glaze according to the firing state of the final sample; wherein the melting temperature range is a temperature range between a preset firing temperature corresponding to the final test in a hemispherical shape and a preset firing temperature corresponding to the final flat sample.

[0075] In specific implementation, the melting temperature range of the compressed glaze can be determined by observing the firing state of the final sample. Specifically, when the edges of the cylindrical sample become rounded, it means that the sample begins to soften. Furthermore, when the cylindrical sample becomes hemispherical, it means that the sample begins to melt. In addition, when the cylindrical sample becomes flat, it means that the sample begins to flow. The melting temperature range is determined based on the shape of the cylindrical sample.

[0076] 4. Flow value

[0077] Specifically, in the present application, the flow value is characterized by the length of the compressed glaze flowing at high temperature. It should be noted that the flow value is mainly determined by the high temperature viscosity of the glaze, and also by the surface tension of the glaze in the molten state.

[0078] Determining the flow value of glaze within the firing range is one of the important items to identify whether glaze and porcelain are suitable. If the flow value of glaze is too large or too small, the product will have defects, such as glaze flow, glaze accumulation, dry glaze, uneven glaze coverage, poor surface gloss, etc.

[0079] There are two methods for measuring flow value, namely the plate method and the chute method. The following uses the plate method as an example to introduce the flow value measurement method.

[0080] It should be noted that when using the plate method to determine the flow value, the instruments and apparatus required include:

[0081] 1. Sieve: one mesh size of 0.15mm (100 mesh standard sieve);

[0082] 2. Metal mold: Φ15×15mm;

[0083] 3. Leveling mud board: (100~130)×(30~60)×(8~10)mm;

[0084] 4. Refractory bearing; inclination angle 20°;

[0085] 5. Vernier caliper; minimum reading 0.02mm;

[0086] 6. Mallet, CMC gel.

[0087] Further, optionally, in a possible implementation, the flow value is measured according to the following method:

[0088] (1) Based on the compressed glaze, a preset number of cylindrical samples of a preset size are prepared according to a high temperature fluidity test sample preparation method.

[0089] Specifically, the preparation of the cylindrical sample is to add CMC gel to the dry glaze powder until the powder is slightly moist. The evenly mixed powder is put into a metal mold with a size of Φ15×15mm and pounded into a Φ15×10mm cylinder. If the sample is too high, sandpaper or a paper cutter can be used to trim the sample height to 10mm. The upper and lower surfaces of the cylindrical sample are required to be flat and have clear edges and corners. The sample is dried to make a cylindrical sample.

[0090] (2) The cylindrical sample is glued to one end of a flat clay plate to obtain an intermediate sample, and the intermediate sample is placed on a refractory support to obtain a final test; wherein the inclination of the refractory support is 20°.

[0091] The size of the flat mud board is about (100-130) × (30-60) × (8-10) mm. In the specific implementation, take the pre-prepared dry mud board and cylindrical sample, apply an appropriate amount of CMC gel on the bottom of the cylindrical sample, and place it in the center of one end of the mud board, and place the mud board on a refractory support inclined at 20°.

[0092] (3) According to the firing system of the electric porcelain blank, the final sample is placed in an electric furnace or a kiln for firing, and a temperature measuring cone is placed in the electric furnace or the kiln.

[0093] (4) The longest length A and the widest width B of the molten final sample are measured, and the sum of A and B is determined as the flow value of the compressed glaze within the firing temperature range.

[0094] Specifically, the flow value is calculated according to the following formula:

[0095] ,

[0096] in, L is the flow value, in mm;

[0097] A It is the length of the longest part of the final specimen, in mm;

[0098] B It is the width of the final specimen at its widest point, in mm.

[0099] 5. Glaze strength

[0100] Optionally, in a possible implementation, the glazing strength is measured by the following method:

[0101] Step 1: Based on the compressed glaze, a rectangular glaze test strip is prepared.

[0102] Among them, the glaze test strip is a small ceramic sample used to test the effect and performance of the glaze on the product surface.

[0103] Specifically, the preparation method of the glazed test strip is as follows:

[0104] (1) Use a small vacuum clay machine to extrude the clay (which can be an electrical porcelain material) into clay strips with a diameter of 23 mm. Repeat the clay kneading process until the clay strips are radially sliced ​​and bent without obvious cracks. Cut the clay strips into test strips about 140 to 180 mm in length, move them to a flat wooden board covered with paper and dry them in the shade for at least 12 hours, and then dry them at 105 to 110°C to a moisture content of less than 1.5%.

[0105] (2) Take out the test strip, cool it to room temperature, and wipe it with a half-wrung-out sponge to remove dust and tiny surface defects on the surface and make the test strip moist.

[0106] (3) Pinch one end with your fingers and place the test strip vertically into the glaze (the compressed glaze provided in this application) for 3 seconds to glaze it. There is about 15 mm of unglazed end on the pinched end; insert the unglazed end of the glazed test strip into the drilled refractory brick, keep it vertical to the refractory brick, and send it into the kiln for firing.

[0107] It should be noted that the outer surface of the fired test strips should be smooth and regular in shape, without streaks, cracks, bubbles, iron impurities, spots and other defects that affect performance. The glaze surface of the glazed sample should be smooth, without defects such as glaze missing, glaze accumulation, glaze sticking, crystallization and uneven color. At least 8 to 10 qualified test strips of each type of unglazed and glazed test strips are provided for testing.

[0108] Step 2: Measure the diameter d of the glazing test strip with a vernier caliper.

[0109] Specifically, the diameter of the test bar is measured in order to calculate the cross-sectional area of ​​the test bar, which is then used in the calculation of flexural strength. Flexural strength is the ability of the test bar to resist damage under bending force, which is usually expressed as the maximum bending stress per unit area. The calculation of bending stress requires the cross-sectional area of ​​the test bar, which can be calculated from the diameter of the test bar.

[0110] Step 3: placing the glazed test strip on a sample holder of an electronic universal material testing machine, and operating the electronic universal material testing machine so that the pressure head of the electronic universal material testing machine applies static pressure to the center of the glazed test strip.

[0111] Specifically, the sample holder is fixed on the workbench of the electronic universal materials testing machine, and its position can be adjusted to accommodate test strips of different sizes. The pressure application speed and application time of the pressure head of the electronic universal materials testing machine can be adjusted according to specific experimental requirements. During the test, the sensors on the electronic universal materials testing machine will monitor the pressure and displacement changes during the test in real time, and store the data in the control system of the electronic universal materials testing machine.

[0112] Step 4: After the glazing test strip is broken, the breaking load F of the glazing test strip is recorded, and the glazing strength is calculated according to the following formula:

[0113] ,

[0114] Among them, the R f is the glazing strength of the glazing test strip, in MPa;

[0115] Said Lis the length of the specimen holder in mm.

[0116] The compressed glaze provided in the present application has been tested on a small sample of the above formula, and the viscosity, glazing strength, melting temperature range, and flow value of the compressed glaze have reached a balance, and the expansion coefficient has been reduced.

[0117] Specific examples and comparative examples are given below to describe the technical solution of the present application in detail:

[0118] Embodiment 1:

[0119] Specifically, the total mass of one portion of compressed glaze is 500 grams. According to weight percentage, Table 1.1 is a formula ratio table of the compressed glaze shown in Example 1 of the present application:

[0120] Table 1.1 Formula ratio of compressed glaze shown in Example 1

[0121] Potassium feldspar Quartz powder Wollastonite Guangxi white clay Washing Faku soil Cordierite powder Barium carbonate Manganese dioxide total Formula ratio / weight percentage 16% 8% 12% 5% 9% 45% 3% 2% 100 Mass / g 80 40 60 25 45 225 15 10 500

[0122] Please refer to Table 1.1. In the example shown in Table 1.1, the chemical composition in the compressed glaze is introduced by 16% potassium feldspar, 8% quartz powder, 12% wollastonite, 5% Guangxi white mud, 9% washed Faku clay, 45% cordierite powder, 3% barium carbonate, and 2% manganese dioxide.

[0123] Further, in the example shown in Table 1.1, the chemical composition of the compressed glaze is shown in Table 1.2:

[0124] Table 1.2 Chemical composition of the compressed glaze shown in Example 1

[0125] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> BaO <![CDATA[MnO2]]> content / % 68.53 14.25 0.47 3.48 3.63 3.64 0.71 0.33 2.21 1.87

[0126] It should be noted that in the example shown in Table 1.2, the loss on ignition of the insulator material is 1.19%. Furthermore, at this time, the measured performance parameters are shown in Table 1.3:

[0127] Table 1.3 Performance parameters of the compressed glaze shown in Example 1

[0128]

[0129] Please refer to Tables 1.1 to 1.3 at the same time. In Example 1, the synergistic effect of potassium feldspar, wollastonite and cordierite powder leads to a balance in viscosity, glazing strength, melting temperature and flow value of the compressed glaze, and reduces the expansion coefficient to less than 4.3 m / °C.

[0130] Embodiment 2:

[0131] Table 2.1 is a formula ratio table of the compressed glaze shown in Example 2 of the present application. Please refer to Table 2.1. The difference between Example 2 and Example 1 lies in the different component contents:

[0132] Table 2.1 Formula ratio of compressed glaze shown in Example 2

[0133] Potassium feldspar Quartz powder Wollastonite Guangxi white clay Washing Faku soil Cordierite powder Barium carbonate Manganese dioxide total Formula ratio / weight percentage 18% 8% 12% 5% 9% 44% 2% 2% 100% Mass / g 80 40 60 25 45 220 10 10 500

[0134] Please refer to Table 2.1. In the example shown in Table 2.1, the chemical composition of the compressed glaze is introduced by 18% potassium feldspar, 8% quartz powder, 12% wollastonite, 5% Guangxi white mud, 9% washed Faku clay, 44% cordierite powder, 2% barium carbonate, and 2% manganese dioxide.

[0135] Further, in the example shown in Table 2.1, the chemical composition of the compressed glaze is shown in Table 2.2:

[0136] Table 2.2 Chemical composition of the compressed glaze shown in Example 2

[0137] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> BaO <![CDATA[MnO2]]> content / % 68.21 14.01 0.44 3.31 3.43 3.91 0.84 0.31 1.51 1.86

[0138] It should be noted that in the example shown in Table 2.2, the loss on ignition of the insulator material is 1.21%. Furthermore, at this time, the measured performance parameters are shown in Table 2.3:

[0139] Table 2.3 Performance parameters of the compressed glaze shown in Example 2

[0140]

[0141] Please refer to Tables 2.1 to 2.3 at the same time. In Example 2, the synergistic effect of potassium feldspar, wollastonite and cordierite powder leads to a balance in the viscosity, glazing strength, melting temperature and flow value of the compressed glaze, and reduces the expansion coefficient to less than 4.3 m / °C.

[0142] Embodiment 3:

[0143] Table 3.1 is a formula ratio table of the compressed glaze shown in Example 3 of the present application. Please refer to Table 3.1. The compressed glaze shown in Example 3 is similar to the compressed glaze shown in the previous embodiment, except that the component contents are different:

[0144] Table 3.1 Formula ratio of compressed glaze shown in Example 3

[0145] Potassium feldspar Quartz powder Wollastonite Guangxi white clay Washing Faku soil Cordierite powder Barium carbonate Manganese dioxide total Formula ratio / weight percentage 14% 8% 12% 7% 8% 45% 4% 2% 100 Mass / g 70 40 60 35 40 225 20 10 500

[0146] Please refer to Table 3.1. In the example shown in Table 3.1, the chemical composition of the compressed glaze is introduced by 14% potassium feldspar, 8% quartz powder, 12% wollastonite, 7% Guangxi white mud, 8% washed Faku clay, 45% cordierite powder, 4% barium carbonate, and 2% manganese dioxide.

[0147] Furthermore, the chemical composition of the compressed glaze is shown in Table 3.2:

[0148] Table 3.2 Chemical composition of the compressed glaze shown in Example 3

[0149] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> BaO <![CDATA[MnO2]]> content / % 67.17 14.57 0.47 3.29 3.52 3.64 0.61 0.27 3.51 1.86

[0150] It should be noted that in the example shown in Table 3.2, the loss on ignition of the insulator material is 1.42%. Furthermore, at this time, the measured performance parameters are shown in Table 3.3:

[0151] Table 3.3 Performance parameters of the compressed glaze shown in Example 3

[0152]

[0153] Please refer to Table 3.1 to Table 3.3 at the same time. In this embodiment, the synergistic effect of potassium feldspar, wollastonite and cordierite powder causes the viscosity, glazing strength, melting temperature and flow value of the compressed glaze to reach a balance, and the expansion coefficient is reduced to less than 4.3 m / °C.

[0154] Embodiment 4:

[0155] Table 4.1 is a formula ratio table of the compressed glaze shown in Example 4 of the present application. Please refer to Table 4.1. The compressed glaze shown in Example 4 is similar to the compressed glaze shown in the previous examples, except that the content of the components is different:

[0156] Table 4.1 Formula ratio of compressed glaze shown in Example 4

[0157] Potassium feldspar Quartz powder Wollastonite Guangxi white clay Washing Faku soil Cordierite powder Barium carbonate Manganese dioxide total Formula ratio / weight percentage 16% 9% 10% 6% 8% 45% 4% 2% 100 Mass / g 80 45 50 30 40 225 20 10 500

[0158] Furthermore, in this example, the chemical composition of the compressed glaze is shown in Table 4.2:

[0159] Table 4.2 Chemical composition of the compressed glaze shown in Example 4:

[0160] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> BaO <![CDATA[MnO2]]> content / % 66.04 14.33 0.44 3.21 3.62 3.71 0.70 0.23 1.68 1.87

[0161] It should be noted that in the example shown in Table 4.2, the loss on ignition of the insulator material is 1.31%. Furthermore, at this time, the measured performance parameters are shown in Table 4.3:

[0162] Table 4.3 Performance parameters of the compressed glaze shown in Example 4

[0163]

[0164] Please refer to Table 4.1 to Table 4.3 at the same time. In this embodiment, the synergistic effect of potassium feldspar, wollastonite and cordierite powder causes the viscosity, glazing strength, melting temperature and flow value of the compressed glaze to reach a balance, and the expansion coefficient is reduced to less than 4.3 m / °C.

[0165] Please refer to Example 1 to Example 4 at the same time. It should be noted that the formula uses washed Faku clay with higher viscosity, reduces the total amount of clay raw materials, increases the amount of barren raw materials to coordinate the melting temperature of the formula and ensure the suspension of the glaze slurry. The aluminum content in the formula is increased to achieve the purpose of ensuring strength, and the magnesium oxide content is increased to achieve the effect of reducing the expansion coefficient; further, the increase in the aluminum content in the formula will lead to an increase in the overall melting temperature, so barium carbonate and manganese dioxide are added to achieve the purpose of reducing the melting temperature of the formula.

[0166] Furthermore, in order to verify the performance of the compressed glaze provided in the present application, the present application also provides some comparative examples, which are described below:

[0167] Comparative Example 1:

[0168] Table 5.1 is a formula ratio table of the compressed glaze shown in Comparative Example 1 of the present application. Please refer to Table 5.1. The difference between Comparative Example 1 and the above embodiment is that the compressed glaze does not contain cordierite powder.

[0169] Table 5.1 Formula ratio of the compressed glaze shown in Comparative Example 1:

[0170] Potassium feldspar Quartz powder Wollastonite Guangxi white clay Washing Faku soil Cordierite powder Barium carbonate Manganese dioxide total Formula ratio / weight percentage 30% 35% 15% 7% 8% —— 3% 2% 100 Mass / g 150 165 75 35 40 —— 15 10 500

[0171] Furthermore, in Comparative Example 1, the chemical composition of the compressed glaze is shown in Table 5.2:

[0172] Table 5.2 Chemical composition of the compressed glaze shown in Comparative Example 1

[0173] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> BaO <![CDATA[MnO2]]> content / % 68.24 12.13 0.42 3.18 3.65 3.75 0.64 0.18 2.21 1.87

[0174] It should be noted that in the example shown in Table 5.2, the loss on ignition of the insulator material is 1.18%. Furthermore, in this example, the measured performance parameters are shown in Table 5.3:

[0175] Table 5.3 Performance parameters of the compressed glaze shown in Comparative Example 1:

[0176]

[0177] Please refer to Table 5.1 to Table 5.3 at the same time. It can be seen that when the glaze formula does not contain cordierite powder, at this time, the melting temperature range and expansion coefficient of the glaze meet the requirements, the viscosity of the glaze is low, the strength is low, and the flow value is large, which does not meet the requirements and it is difficult to achieve a balance between viscosity, glazing strength, melting temperature and flow value.

[0178] Comparative Example 2:

[0179] Table 6.1 is a formula ratio table of the compressed glaze shown in Comparative Example 2 of the present application. Please refer to Table 6.1. The difference between Comparative Example 2 and the above embodiment is that the cordierite powder in the compressed glaze is replaced with burned talc.

[0180] Table 6.1 Formula ratio of compressed glaze shown in Comparative Example 2

[0181] Potassium feldspar Quartz powder Wollastonite Guangxi white clay Washing Faku soil Burnt Talc Barium carbonate Manganese dioxide total Formula ratio / weight percentage 14% 8% 12% 7% 8% 45% 4% 2% 100 Mass / g 70 40 60 35 40 225 20 10 500

[0182] Furthermore, in Comparative Example 2, the chemical composition of the compressed glaze is shown in Table 6.2:

[0183] Table 6.2 Chemical composition of the compressed glaze shown in Comparative Example 2

[0184] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> BaO <![CDATA[MnO2]]> content / % 67.31 10.21 0.31 3.18 8.33 3.54 0.51 0.31 3.18 1.84

[0185] It should be noted that in the example shown in Table 6.2, the loss on ignition of the insulator material is 1.54%. Furthermore, the measured performance parameters are shown in Table 6.3:

[0186] Table 6.3 Performance parameters of the compressed glaze shown in Comparative Example 2

[0187]

[0188] Please refer to Tables 6.1 to 6.3 at the same time. It can be seen that when the cordierite powder in the compressed glaze is replaced by burned talc, the melting temperature and expansion coefficient of the compressed glaze meet the requirements, but the viscosity of the glaze is lower, the strength is lower, and the flow value is larger, which does not meet the requirements and it is difficult to achieve a balance between viscosity, glazing strength, melting temperature and flow value.

[0189] Comparative Example 3:

[0190] Table 7.1 is a formula ratio table of the compressed glaze shown in Comparative Example 3 of the present application. Please refer to Table 7.1. The difference between Comparative Example 3 and the above-mentioned embodiment is that the content of cordierite powder exceeds the set range.

[0191] Table 7.1 Formula ratio of compressed glaze shown in comparative example 3

[0192] Potassium feldspar Quartz powder Wollastonite Guangxi white clay Washing Faku soil Cordierite powder Barium carbonate Manganese dioxide total Formula ratio / weight percentage 14% 5% 12% 6% 6% 51% 4% 2% 100 Mass / g 70 25 60 30 30 255 20 10 500

[0193] At this time, in the example shown in Table 7.1, the chemical composition of the compressed glaze is shown in Table 7.2:

[0194] Table 7.2 Chemical composition of the compressed glaze shown in Comparative Example 3

[0195] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> BaO <![CDATA[MnO2]]> content / % 65.87 17.38 0.29 3.32 4.89 3.62 0.70 0.22 3.14 1.85

[0196] It should be noted that in the example shown in Table 7.2, the loss on ignition of the insulator material is 1.21%. Furthermore, at this time, the measured performance parameters are shown in Table 7.3:

[0197] Table 7.3 Performance parameters of the compressed glaze shown in Comparative Example 3

[0198]

[0199] Please refer to Table 7.1 to Table 7.3. It can be seen that in Comparative Example 3, when the content of cordierite powder exceeds the set range, the melting temperature and expansion coefficient of the compressed glaze meet the requirements, the viscosity of the glaze is low, the strength is low, and the flow value is large, which does not meet the requirements and it is difficult to achieve a balance between viscosity, glazing strength, melting temperature and flow value.

[0200] In summary, Table 8.1 is a formula ratio table corresponding to each of the above embodiments, Table 8.2 is a chemical composition table corresponding to each of the above embodiments, and Table 8.3 is a performance parameter table corresponding to each of the above embodiments:

[0201] Table 8.1 Formula ratio table corresponding to each embodiment

[0202] formula Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Potassium feldspar 16% 18% 14% 16% 30% 14% 14% Quartz powder 8% 8% 8% 9% 35% 8% 5% Wollastonite 12% 12% 12% 10% 15% 12% 12% Guangxi white clay 5% 5% 7% 6% 7% 7% 6% Washing Faku soil 9% 9% 8% 8% 8% 8% 6% Cordierite powder 45% 44% 45% 45% —— —— 51% Barium carbonate 3% 2% 4% 4% 3% 4% 4% Manganese dioxide 2% 2% 2% 2% 2% 2% 2% Burnt Talc —— —— —— —— —— 45% ——

[0203] Table 8.2 Chemical components corresponding to various examples

[0204] Chemical composition Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[SiO2]]> 68.53 68.21 67.17 66.04 68.24 67.31 65.87 <![CDATA[Al2O3]]> 14.25 14.01 14.57 14.33 12.13 10.21 17.38 <![CDATA[Fe2O3]]> 0.47 0.44 0.47 0.44 0.42 0.31 0.29 CaO 3.48 3.31 3.29 3.21 3.18 3.18 3.32 MgO 3.63 3.43 3.52 3.62 3.65 8.33 4.89 <![CDATA[K2O]]> 3.64 3.91 3.64 3.71 3.75 3.54 3.62 <![CDATA[Na2O]]> 0.71 0.84 0.61 0.70 0.64 0.51 0.70 <![CDATA[TiO2]]> 0.33 0.31 0.27 0.23 0.18 0.31 0.22 BaO 2.21 1.51 3.51 1.68 2.21 3.18 3.14 <![CDATA[MnO2]]> 1.87 1.86 1.86 1.87 1.87 1.84 1.85

[0205] Table 8.3 Performance parameters corresponding to various embodiments

[0206] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Viscosity 1862 1755 2011 1964 1548 1574 1612 Unglazed Strength 162 162 161 163 162 161 161 Glaze strength 191 192 194 195 170 150 164 Melting temperature 1160~1240 1150~1220 1150~1220 1160~1240 1120~1180 1120~1180 1140~1200 Flow value 53.41 59.12 58.67 56.84 69.23 69.42 57.45 Expansion coefficient 3.8864 3.7652 3.66337 3.6334 3.7448 3.9667 3.7457

[0207] Please refer to Tables 8.1 to 8.3. It can be seen that in the present application, SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O, TiO2, BaO, and MnO2 are introduced into the compressed glaze by utilizing 14% to 18% potassium feldspar, 6% to 10% quartz powder, 10% to 14% wollastonite, 3% to 7% Guangxi white mud, 7% to 11% washed Faku clay, 43% to 47% cordierite powder, 1% to 5% barium carbonate, and 1% to 3% manganese dioxide. In this way, through the synergistic effect of potassium feldspar, wollastonite and cordierite powder, the viscosity, glazing strength, melting temperature and flow value of the compressed glaze can be balanced, and the expansion coefficient can be reduced.

[0208] Specifically, potassium feldspar is a flux, and the potassium ions in potassium feldspar can enhance the fluidity of the glaze in the molten state, which helps to evenly distribute the glaze layer. In addition, during the sintering process, potassium feldspar can form a glass phase to enhance the mechanical strength of the glaze layer; further, wollastonite has good chemical stability at high temperatures and can stabilize the melting behavior of the glaze; in addition, the crystal structure of wollastonite can increase the mechanical strength of the glaze layer and prevent cracks and peeling; further, cordierite has excellent thermal stability and can improve the stability and thermal shock resistance of the glaze at high temperatures; in addition, cordierite powder can adjust the viscosity of the glaze, making it easy to control during the glazing process. It should be noted that wollastonite and cordierite powder have low expansion coefficients, which can effectively reduce the overall expansion coefficient of the glaze and reduce thermal stress.

[0209] Relevant explanations on the synergistic effect: First, potassium feldspar, as a flux, can reduce the melting temperature and viscosity of the glaze, while wollastonite and cordierite powder can provide a certain balance of structure and viscosity, so that the glaze has appropriate viscosity when glazing, and is easy to control and apply; second, the glass phase formed by potassium feldspar during the firing process can enhance the strength of the glaze layer, while the structural support provided by wollastonite and cordierite powder can improve the mechanical strength of the glaze layer, so that the glaze has a higher glazing strength and avoids cracking and peeling; third, while potassium feldspar reduces the melting temperature, wollastonite and cordierite powder ensure that the glaze melts and flows within the appropriate temperature range, and will not cause excessive flow due to too low a melting temperature, or be difficult to melt due to too high a melting temperature; fourth, potassium feldspar can improve fluidity and ensure that the glaze can be evenly covered in a molten state, while wollastonite and cordierite powder can adjust this fluidity so that the glaze does not flow excessively during the melting process, thereby forming a uniform and appropriately thick glaze layer.

[0210] In addition, both wollastonite and cordierite powder have low expansion coefficients. By introducing wollastonite and cordierite powder, the overall expansion coefficient of the glaze is significantly reduced, reducing the stress and cracks caused by thermal expansion mismatch during heat treatment.

[0211] In summary, the compressed glaze provided in the present application, through the synergistic enhancement of potassium feldspar, wollastonite and cordierite powder, can balance the viscosity, glazing strength, melting temperature and flow value of the compressed glaze, and reduce the expansion coefficient. Furthermore, when the viscosity, glazing strength, melting temperature and flow value are balanced, it can not only ensure that the glaze exhibits excellent operating performance during glazing and firing, but also ensure the high-quality surface of the final product, so that it has good mechanical strength, smoothness and durability, thereby meeting the high standards required in practical applications.

[0212] Furthermore, in order to verify the product performance, glaze sand was produced in the blank making workshop, and test products were made according to the normal production process. The destructive strength of the test products was tested. The test results are shown in Tables 9, 10, and 11. Among them, when testing the destructive strength, the product's failure form was the extension of the steel foot.

[0213] Specifically, the destructive strength of the 210kN product is shown in Table 9:

[0214] Table 9

[0215]

[0216] Similarly, the destructive strength of the 420kN product is shown in Table 10:

[0217] Table 10

[0218]

[0219] Similarly, the destructive strength of the 160kN product is shown in Table 11:

[0220] Table 11

[0221]

[0222] Please refer to Table 9, Table 10 and Table 11 at the same time. The destructive strength of all types of test products can reach the rated strength.

[0223] Furthermore, the present application also provides a method for preparing a compressed glaze slurry. The following is an introduction to the method for preparing a compressed glaze slurry provided in the present application:

[0224] Figure 1 This is a flow chart of Example 1 of the method for preparing compressed glaze slurry provided in this application. Figure 1 The method for preparing a compressed glaze slurry provided in this embodiment is used to prepare a compressed glaze slurry using any of the compressed glaze materials provided in the first aspect of the present application, and the method comprises:

[0225] S101, hydrating the potassium feldspar, quartz powder, wollastonite, cordierite powder, barium carbonate and manganese dioxide in the compressed glaze to obtain a first mixed slurry.

[0226] It is understood that the potassium feldspar, quartz powder, wollastonite, cordierite powder, barium carbonate and manganese dioxide in the compressed glaze are powdered materials, wherein the particle size of potassium feldspar, quartz powder, wollastonite, cordierite powder and barium carbonate is less than 200 mesh (screen residue <3%), and the particle size of manganese dioxide is less than 320 mesh (can pass through a 320 mesh sieve). When preparing the glaze slurry, the potassium feldspar, quartz powder, wollastonite, cordierite powder, barium carbonate and manganese dioxide in the compressed glaze need to be hydrated to obtain a first mixed slurry.

[0227] S102, using a ball mill to perform a ball milling operation on the mixed slurry, Guangxi white mud and washed Faku soil in the compressed glaze to obtain a second mixed slurry.

[0228] Specifically, deionized water is added as a medium during the ball milling process to avoid the influence of calcium and magnesium ions in the water. After ball milling, the mixture is sieved through a 325-mesh sieve to ensure that the residue is controlled between 0.06% and 0.12%.

[0229] S103, filtering the first mixed slurry to obtain filtered slurry.

[0230] In a specific implementation, the first mixed slurry can be filtered through a mesh screen to remove impurities and large particles. For example, in one embodiment, the first mixed slurry can be filtered through two sieves, the two sieves are a 200 mesh sieve and a 240 mesh sieve.

[0231] S104, performing iron removal treatment on the filtered slurry.

[0232] In specific implementation, a 12000 Gauss wet iron remover can be used to remove iron from the filtered slurry. In specific implementation, the first mixed slurry flows directly into the corresponding second vibrating screen through a screened glaze slurry, and then enters the primary slurry storage tank after passing through the second vibrating screen. After being stirred evenly, it is pumped into the corresponding Gauss wet iron remover with a pneumatic diaphragm pump for iron removal, and then flows into the fine material tank.

[0233] The present embodiment provides a method for preparing compressed glaze slurry. By this method, compressed glaze slurry can be prepared so that the viscosity, glazing strength, melting temperature and flow value of the compressed glaze slurry are balanced. Furthermore, on the basis of ensuring the balance of various performance parameters, the expansion coefficient is reduced.

[0234] The third aspect of the present application further provides an insulator, the head of which is glazed based on the compressed glaze slurry provided in the second aspect of the present application.

[0235] The benefits of using compressed glaze on insulators are mainly reflected in improving insulation performance, enhancing weather resistance, improving mechanical strength, preventing pollution accumulation, improving corrosion resistance, aesthetics and reducing maintenance costs. The dense glaze layer formed by compressed glaze can effectively reduce tiny pores and cracks, improve the surface strength and wear resistance of the insulator, resist the influence of the external environment, extend the service life of the insulator, and reduce maintenance costs.

[0236] The insulator provided in the present application can improve its mechanical strength based on the compressed glaze slurry glazing, and can ensure the controllability of the glazing operation and improve the surface quality of the product.

[0237] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A compressed glaze based on cordierite powder, It is characterized in that The compressed glaze comprises the following chemical components: SiO 2 、Al 2 O 3 , Fe 2 O 3 , CaO, MgO, K 2 O、Na 2 O、TiO 2 、BaO、MnO 2 ; According to weight percentage, the chemical components in the compressed glaze are introduced by 14% to 18% potassium feldspar, 6% to 10% quartz powder, 10% to 14% wollastonite, 3% to 7% Guangxi white mud, 7% to 11% washed Faku clay, 43% to 47% cordierite powder, 1% to 5% barium carbonate, and 1% to 3% manganese dioxide; The synergistic effect of potassium feldspar, wollastonite and cordierite powder in the compressed glaze leads to a balance in viscosity, glazing strength, melting temperature and flow value of the compressed glaze, and reduces the expansion coefficient.

2. The compressed glaze based on cordierite powder according to claim 1, It is characterized in that The compressed glaze comprises the following chemical components: 68.53% SiO 2 , 14.25% Al 2 O 3 , 0.47% Fe 2 O 3 , 3.48% CaO, 3.63% MgO, 3.64% K 2 O, 0.71%Na 2 O, 0.33% TiO 2 , 2.21%BaO, 1.87%MnO 2 ; The chemical components in the compressed glaze are introduced by 16% potassium feldspar, 8% quartz powder, 12% wollastonite, 5% Guangxi white mud, 9% washed Faku clay, 45% cordierite powder, 3% barium carbonate, and 2% manganese dioxide.

3. The compressed glaze according to claim 1, It is characterized in that The compressed glaze comprises the following chemical components: 68.21% SiO 2 , 14.01% Al 2 O 3 , 0.44% Fe 2 O 3 , 3.31% CaO, 3.43% MgO, 3.91% K 2 O, 0.84%Na 2 O, 0.31% TiO 2 , 1.51%BaO, 1.86%MnO 2 ; The chemical components in the compressed glaze are introduced by 18% potassium feldspar, 8% quartz powder, 12% wollastonite, 5% Guangxi white mud, 9% washed Faku clay, 44% cordierite powder, 2% barium carbonate, and 2% manganese dioxide.

4. The compressed glaze according to claim 1, It is characterized in that The compressed glaze comprises the following chemical components: 67.17% SiO 2 , 14.57% Al 2 O 3 , 0.47% Fe 2 O 3 , 3.29% CaO, 3.52% MgO, 3.64% K 2 O, 0.61%Na 2 O, 0.27% TiO 2 , 1.86%BaO, 1.86%MnO 2 ; The chemical components in the compressed glaze are introduced by 14% potassium feldspar, 8% quartz powder, 12% wollastonite, 7% Guangxi white mud, 8% washed Faku clay, 45% cordierite powder, 4% barium carbonate, and 2% manganese dioxide.

5. The compressed glaze according to claim 1, It is characterized in that The compressed glaze comprises the following chemical components: 66.04% SiO 2 , 14.33% Al 2 O 3 , 0.44% Fe 2 O 3 , 3.21% CaO, 3.62% MgO, 3.71% K 2 O, 0.70%Na 2 O, 0.23% TiO 2 , 1.68%BaO, 1.87%MnO 2 ; The chemical components in the compressed glaze are introduced by 16% potassium feldspar, 9% quartz powder, 10% wollastonite, 6% Guangxi white mud, 8% washed Faku clay, 45% cordierite powder, 4% barium carbonate, and 2% manganese dioxide.

6. The compressed glaze according to claim 1, It is characterized in that The total mass of the compressed glaze is 500 g.

7. The compressed glaze according to claim 1, It is characterized in that The particle sizes of the potassium feldspar, quartz powder, wollastonite, cordierite powder and barium carbonate are less than 200 meshes; and the particle size of the manganese dioxide is less than 320 meshes.

8. A method for preparing a compressed glaze slurry, It is characterized in that The method uses the compressed glaze material according to any one of claims 1 to 7 to prepare the compressed glaze slurry; the method comprises: Hydration treatment is performed on the potassium feldspar, quartz powder, wollastonite, cordierite powder, barium carbonate and manganese dioxide in the compressed glaze to obtain a first mixed slurry; Using a ball mill to perform a ball milling operation on the first mixed slurry, Guangxi white mud and washed Faku soil in the compressed glaze to obtain a second mixed slurry; filtering the second mixed slurry to obtain filtered slurry; The filtered slurry is subjected to iron removal treatment to obtain the compressed glaze slurry.

9. The preparation method according to claim 8, It is characterized in that The ball milling operation uses deionized water as the medium.

10. An insulator, It is characterized in that The head of the insulator is glazed based on the compressed glaze slurry according to claim 8.