A self-supporting positive electrode material for lithium-sulfur batteries and its preparation method and application
By introducing europium-doped nickel selenide catalyst and carbon nanofibers into the cathode material of lithium-sulfur batteries, the problems of volume expansion and polysulfide shuttle effect of lithium-sulfur batteries are solved, and high-capacity and cycle-stable lithium-sulfur battery performance are achieved. , promoting its application in energy storage systems.
Patent Information
- Application Number
- CN202411006742.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Due to problems such as the poor conductivity of sulfur, the volume expansion of the cathode material during charge and discharge, and the polysulfide shuttle effect, lithium-sulfur batteries limit the actual capacity retention rate and overall performance of the battery, hindering its widespread use in energy storage systems. application.
Electrospinning technology is used to prepare self-supporting cathode materials for lithium-sulfur batteries. Europium-doped nickel selenide (NiSe) catalyst is introduced into carbon nanofibers to form NiSe-Eu@CNF, which improves the polarity and catalytic activity of the material and limits Shuttling effect of polysulfides and mitigating volume expansion through the conductive network of carbon nanofibers.
The lithium-sulfur battery that has achieved high specific capacity and high cycle stability can operate stably under high loads, with a discharge capacity of 896.2 mAh·g-1, and it still has 657.8 mAh·g-1 after 500 cycles at a current density of 1 C. The capacity of g-1 has practical application value.
Smart Images

Figure CN118531530B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-sulfur battery positive electrode materials, and in particular to a self-supporting positive electrode material for lithium-sulfur batteries and a preparation method and application thereof. Background Art
[0002] Lithium-sulfur batteries based on electrochemical reaction conversion mechanisms have great potential to become the next generation of energy storage systems due to their advantages such as high theoretical specific capacity, high energy density, low cost and environmental friendliness. However, the existence of various problems such as the poor conductivity of sulfur and its discharge products, the nearly 80% volume expansion of the positive electrode material during the charging and discharging process, and the "shuttle effect" of the intermediate product polysulfide have greatly limited the actual capacity retention rate and overall performance of the battery, thus hindering the pace of lithium-sulfur batteries to fully replace lithium-ion batteries. Therefore, it is urgent to find and develop a suitable lithium-sulfur battery positive electrode material to alleviate the above problems, in order to fully release the potential of lithium-sulfur batteries and promote their commercial application.
[0003] In recent years, researchers have conducted many studies on the above issues, such as constructing suitable carrier materials to confine sulfur active substances in a three-dimensional structure with good conductivity. On the one hand, the good conductive framework of the carrier material can provide a smooth electron-mediated pathway for sulfur redox reactions, and on the other hand, the composite material itself has a large pore volume that can effectively alleviate the volume expansion of sulfur; or further introduce catalysts into the host material, and limit the migration of polysulfides between the positive and negative electrodes through a combination of multiple strategies such as physical confinement, chemical adsorption, and accelerating the conversion rate of intermediate polysulfides. However, the above lithium-sulfur battery positive electrode materials often need to add a large proportion of conductive agents and binders during the preparation process to enhance the conductivity and structural stability of the positive electrode, and the production cost and process are complicated.
[0004] Therefore, designing and developing carrier positive electrode materials that integrate multiple functions is the core link in promoting the development of high-performance lithium-sulfur battery technology. Self-supporting positive electrode materials can directly load active substances as lithium-sulfur battery positive electrodes without adding additional conductive agents and binders, and have unique advantages in electrode stability and increasing sulfur loading. It is easier to prepare thick electrodes with certain flexibility, thereby improving the energy density of the battery. At present, research on self-supporting positive electrode materials for lithium-sulfur batteries focuses on carbonaceous frameworks with microporous and porous structures. Although the current self-supporting positive electrode materials have greatly improved the physical confinement effect of polysulfides, the low chemical activity and non-polarity of carbon itself lead to limited chemical effects on polysulfides. CN110438798A discloses a method of preparing lithium-sulfur battery positive electrode materials by configuring polymethyl methacrylate and polyacrylonitrile into a mixed solution using electrospinning technology. The electrospinning prepared by this method has insufficient mechanical strength and cannot effectively suppress the volume expansion of sulfur during charging and discharging. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a self-supporting positive electrode material for lithium-sulfur batteries and a preparation method and application thereof.
[0006] The above object of the present invention is achieved through the following technical solutions:
[0007] The first aspect of the present invention provides a method for preparing a self-supporting positive electrode material for a lithium-sulfur battery, comprising the following steps:
[0008] (1) dissolving polyacrylonitrile (PAN), nickel salt and europium salt in N,N-dimethylformamide (DMF), stirring evenly to obtain an electrospinning solution, wherein the molar ratio of the nickel salt to the europium salt is (10-20):1;
[0009] (2) electrospinning the electrospinning solution obtained in step (1) to obtain nanofibers;
[0010] (3) The nanofibers obtained in step (2) are subjected to a pre-oxidation treatment, and the pre-oxidation nanofibers are subjected to a carbonization treatment in a selenium vapor atmosphere to obtain the self-supporting positive electrode material for a lithium-sulfur battery.
[0011] The present invention introduces a new europium (Eu)-doped nickel selenide (NiSe) catalyst on the basis of the carbon self-supporting positive electrode material in the prior art to obtain the lithium-sulfur battery self-supporting positive electrode material NiSe-Eu@CNF, which improves the overall polarity of the electrode material, is beneficial to the chemical adsorption of polysulfides, and further enhances the catalytic activity of the material, better limits the shuttle effect of polysulfides, and thus improves the electrochemical performance of the lithium-sulfur battery.
[0012] At the microstructural level, the one-dimensional conductive network formed by the interweaving of carbon nanofibers can effectively improve the transmission efficiency of lithium ions and electrons, and alleviate the problem of large volume strain during the cycle; at the same time, the surface-loaded nanoscale NiSe-Eu is conducive to the full exposure of the active sites of the catalyst, thereby improving the utilization rate of the catalyst.
[0013] At the electronic structure level, Eu doping simultaneously activates the catalytic activity of the metal active site Ni and the non-metal active site Se, so that Eu-doped NiSe has a dual chemical binding effect on polysulfides, produces a strong adsorption effect, and significantly enhances the catalytic activity of the NiSe catalyst.
[0014] The method of preparing self-supporting positive electrode materials by electrospinning technology in the present invention has the advantages of low cost, controllable morphology, easy adjustment of components, and stable structure. The activity of the metal and non-metal centers of the transition metal catalyst is synergistically improved through single doping, providing a new reference for the design of lithium-sulfur battery catalysts with high specific capacity, high energy density and long cycle life.
[0015] Furthermore, in step (1), the molecular weight of the polyacrylonitrile is 149000~151000 Da.
[0016] Furthermore, in step (1), the concentration of polyacrylonitrile in the electrospinning solution is 50-200 mg / mL, and the sum of the concentrations of nickel salt and europium salt in the electrospinning solution is 40-80 mM.
[0017] Furthermore, in step (1), the nickel salt is selected from one or more of nickel nitrate, nickel chloride and nickel sulfate, such as Ni(NO3)2·6H2O, NiCl2·6H2O, NiSO4.
[0018] Furthermore, in step (1), the europium salt is europium chloride and / or europium acetate, such as EuCl3·6H2O, Eu(C2H3O2)3·4H2O.
[0019] Furthermore, in step (1), the molar ratio of the nickel salt to the europium salt is preferably (10-15):1, more preferably (11-13):1.
[0020] Furthermore, in step (1), the stirring is performed at 50-70°C.
[0021] Furthermore, in step (2), the electrospinning conditions are as follows: spinning distance is 13-18 cm, spinning voltage is 13-15 kV, and spinning speed is 0.8-1.1 mL / h.
[0022] Furthermore, in step (3), the pre-oxidation treatment is specifically: placing the nanofibers in a heating device, heating the temperature to 210-230°C at a rate of 1-3°C / min, and keeping the temperature for 2-4 hours.
[0023] Furthermore, in step (3), the carbonization treatment is carried out in a tubular furnace, the selenium powder is placed upstream of the tubular furnace, and the nanofibers after the pre-oxidation treatment are placed downstream of the tubular furnace.
[0024] Furthermore, in step (3), the mass ratio of the selenium powder to the pre-oxidized nanofibers is (3-20):1, preferably (3-10):1, and more preferably (3-5):1.
[0025] Furthermore, in step (3), the carbonization treatment is specifically as follows: firstly heating the temperature to 500-600°C at a rate of 1-3°C / min and keeping the temperature for 1-2 h, then heating the temperature to 800-1000°C at a rate of 5-7°C / min and keeping the temperature for 2-4 h.
[0026] The second aspect of the present invention provides a self-supporting positive electrode material for a lithium-sulfur battery prepared by the method described in the first aspect.
[0027] A third aspect of the present invention provides a lithium-sulfur battery, comprising the self-supporting positive electrode material for a lithium-sulfur battery according to the second aspect.
[0028] The lithium-sulfur battery is assembled from the lithium-sulfur battery self-supporting positive electrode material, negative electrode sheet, separator, active material and ether electrolyte provided by the invention.
[0029] Furthermore, the self-supporting positive electrode material of the lithium-sulfur battery is bonded to the diaphragm, and the other side of the diaphragm is bonded to the negative electrode sheet. The self-supporting positive electrode material of the lithium-sulfur battery, the diaphragm, and the negative electrode sheet bonded as one are sealed in the battery housing as a whole.
[0030] Furthermore, the material of the diaphragm is selected from one or more of polypropylene, polyethylene, polyvinylidene fluoride-hexafluoropropylene copolymer and polypropylene-methyl methacrylate.
[0031] Furthermore, the active material is Li2S6.
[0032] Furthermore, the ether electrolyte is prepared by dissolving lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) in a mixed solution of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a volume ratio of 1:(1~2), and the concentration of LiTFSI in the ether electrolyte is 1~5 mol / L.
[0033] Thanks to the cleverly designed microstructure and optimized electronic structure of the positive electrode material, the self-supporting positive electrode material for lithium-sulfur batteries of the present invention can be used to assemble lithium-sulfur batteries with high specific capacity and high cycle stability, thereby achieving stable operation under high load and having greater practical application value.
[0034] Beneficial effects of the present invention:
[0035] 1. The method of preparing a self-supporting cathode material by electrospinning technology in the present invention has the advantages of low cost, controllable morphology, easy adjustment of components, stable structure, etc. On the basis of the carbon self-supporting cathode material in the prior art, a new catalyst of nickel selenide (NiSe) doped with europium (Eu) is introduced. The activity of the metal and non-metal centers of the transition metal catalyst is synergistically improved through single doping, and the self-supporting cathode material NiSe-Eu@CNF for lithium-sulfur batteries is obtained, which improves the overall polarity and catalytic activity of the electrode material, better limits the shuttle effect of polysulfides, and thus improves the electrochemical performance of lithium-sulfur batteries.
[0036] 2. Thanks to the cleverly designed microstructure and optimized electronic structure of the cathode material, the self-supporting cathode material for lithium-sulfur batteries of the present invention can be used to assemble lithium-sulfur batteries with high specific capacity and high cycle stability, achieving stable operation under high loads and having more practical application value. The lithium-sulfur battery has a high specific capacity and high cycle stability at 4 C (1 C = 1675 mA·g -1 ) at a current density of 896.2 mAh·g -1 The high discharge capacity is 657.8 mAh g after 500 cycles at a current density of 1 C. -1 Even when the sulfur loading reaches 5.94 mg·cm -2 The assembled lithium-sulfur battery can still obtain 5.68 mAh cm -2 The high reversible capacity can be stably cycled 100 times. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The morphology characterization pictures of NiSe-Eu@CNF prepared in Example 1; wherein (a) is a scanning electron microscope picture, (b) is a transmission electron microscope picture, and (c) is a high-resolution transmission electron microscope picture.
[0038] Figure 2 The morphology characterization pictures of NiSe@CNF prepared in comparative example 1; wherein (a) is a scanning electron microscope picture, (b) is a transmission electron microscope picture, and (c) is a high-resolution transmission electron microscope picture.
[0039] Figure 3 This is the EDS mapping image of NiSe-Eu@CNF prepared in Example 1.
[0040] Figure 4 XRD diagrams of NiSe-Eu@CNF prepared in Example 1 and NiSe@CNF prepared in Comparative Example 1.
[0041] Figure 5 This is the XRD diagram of the self-supporting positive electrode material for lithium-sulfur battery prepared in Comparative Example 2.
[0042] Figure 6 The graphs show the adsorption test results of Li2S6 by NiSe-Eu@CNF prepared in Example 1 and NiSe@CNF prepared in Comparative Example 1; wherein (a) is a picture of Li2S6 solution and the solution after adsorption by NiSe-Eu@CNF and NiSe@CNF, respectively; (b) is a picture of UV-Vis spectra of Li2S6 solution and the solution after adsorption by NiSe-Eu@CNF and NiSe@CNF, respectively.
[0043] Figure 7K-edge absorption spectra of Ni and Se before and after the NiSe-Eu@CNF prepared in Example 1 and the NiSe@CNF prepared in Comparative Example 1 adsorbed Li2S6; wherein, (a) is the K-edge absorption spectrum of Ni before and after the NiSe-Eu@CNF adsorbed Li2S6, (b) is the K-edge absorption spectrum of Ni before and after the NiSe@CNF adsorbed Li2S6, (c) is the K-edge absorption spectrum of Se before and after the NiSe-Eu@CNF adsorbed Li2S6, and (d) is the K-edge absorption spectrum of Se before and after the NiSe@CNF adsorbed Li2S6.
[0044] Figure 8 This is a cycling performance diagram of a lithium-sulfur battery assembled with NiSe-Eu@CNF prepared in Example 1 and NiSe@CNF prepared in Comparative Example 1 at 0.2 C.
[0045] Fig. 9 This is the rate performance diagram of the lithium-sulfur battery assembled with NiSe-Eu@CNF prepared in Example 1.
[0046] Fig.10 This is the long cycle performance diagram of the lithium-sulfur battery assembled with NiSe-Eu@CNF prepared in Example 1 at 1 C.
[0047] Fig.11 The sulfur loading of NiSe-Eu@CNF prepared in Example 1 is 5.94 mg·cm -2 Cycling performance diagram of lithium-sulfur battery at a current density of 0.05 C. DETAILED DESCRIPTION
[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0049] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0050] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified. Example 1
[0051] A method for preparing a self-supporting positive electrode material NiSe-Eu@CNF for a lithium-sulfur battery comprises the following steps:
[0052] (1) 1000 mg of polyacrylonitrile, 0.462 mmol Ni(CH3COO)2·4H2O and 0.0385 mmol Eu(C2H3O2)3·4H2O were dissolved in 10 mL N,N-dimethylformamide (DMF) (the molar ratio of Ni(CH3COO)2·4H2O to Eu(C2H3O2)3·4H2O was 12:1) and stirred in an oil bath at 60 °C for 12 h to form a uniform electrospinning solution.
[0053] (2) The electrospinning solution obtained in step (1) was transferred to a plastic syringe with a 21 G needle for electrospinning. The spinning distance between the syringe needle and the collector was 15 cm, the spinning voltage was 14 kV, the spinning speed was 1 mL / h, and the air humidity was 40%, thereby obtaining nanofibers.
[0054] (3) The nanofibers obtained in step (2) were pre-oxidized, heated to 220 °C at a rate of 1 °C / min in a muffle furnace and kept warm for 2 h; 500 mg of selenium powder was placed upstream of the tube furnace, and 150 mg of the pre-oxidized nanofibers were placed downstream of the tube furnace, first heated to 550 °C at a rate of 2 °C / min and kept warm for 1 h, and then heated to 900 °C at a rate of 5 °C / min and kept warm for 2 h, to obtain NiSe-Eu@CNF, a self-supporting positive electrode material for lithium-sulfur batteries. Example 2
[0055] A method for preparing a self-supporting positive electrode material NiSe-Eu@CNF for a lithium-sulfur battery comprises the following steps:
[0056] (1) 1000 mg of polyacrylonitrile, 0.4 mmol NiCl2·6H2O and 0.04 mmol EuCl3·6H2O were dissolved in 10 mL N,N-dimethylformamide (DMF) (the molar ratio of NiCl2·6H2O to EuCl3·6H2O was 10:1) and stirred in an oil bath at 60 °C for 12 h to form a uniform electrospinning solution.
[0057] (2) The electrospinning solution obtained in step (1) was transferred to a plastic syringe with a 21 G needle for electrospinning. The spinning distance between the syringe needle and the collector was 13 cm, the spinning voltage was 15 kV, the spinning speed was 0.8 mL / h, and the air humidity was 40%, thereby obtaining nanofibers.
[0058] (3) The nanofibers obtained in step (2) were pre-oxidized, heated to 230 °C in a muffle furnace at a rate of 2 °C / min and kept warm for 4 h; 1500 mg of selenium powder was placed upstream of the tube furnace, and 150 mg of the pre-oxidized nanofibers were placed downstream of the tube furnace, first heated to 600 °C at a rate of 3 °C / min and kept warm for 2 h, and then heated to 1000 °C at a rate of 5 °C / min and kept warm for 4 h, to obtain NiSe-Eu@CNF, a self-supporting positive electrode material for lithium-sulfur batteries. Example 3
[0059] A method for preparing a self-supporting positive electrode material NiSe-Eu@CNF for a lithium-sulfur battery comprises the following steps:
[0060] (1) 2000 mg of polyacrylonitrile, 0.6 mmol NiSO4 and 0.03 mmol Eu(C2H3O2)3·4H2O were dissolved in 10 mL N,N-dimethylformamide (DMF) (the molar ratio of NiSO4 to Eu(C2H3O2)3·4H2O was 20:1) and stirred in an oil bath at 60 °C for 12 h to form a uniform electrospinning solution.
[0061] (2) The electrospinning solution obtained in step (1) was transferred to a plastic syringe with a 21 G needle for electrospinning. The spinning distance between the syringe needle and the collector was 18 cm, the spinning voltage was 13 kV, the spinning speed was 1.1 mL / h, and the air humidity was 40% to obtain nanofibers.
[0062] (3) The nanofibers obtained in step (2) were pre-oxidized, heated to 210 °C at a rate of 3 °C / min in a muffle furnace and kept warm for 2 h; 500 mg of selenium powder was placed upstream of the tube furnace, and 150 mg of the pre-oxidized nanofibers were placed downstream of the tube furnace, first heated to 500 °C at a rate of 2 °C / min and kept warm for 1 h, and then heated to 800 °C at a rate of 7 °C / min and kept warm for 2 h, to obtain NiSe-Eu@CNF, a self-supporting positive electrode material for lithium-sulfur batteries. Comparative Example 1
[0063] A method for preparing a self-supporting positive electrode material NiSe@CNF for a lithium-sulfur battery comprises the following steps:
[0064] (1) 1000 mg of polyacrylonitrile and 0.5 mmol of Ni(CH3COO)2·4H2O were dissolved in 10 mL of N,N-dimethylformamide (DMF) and stirred in an oil bath at 60 °C for 12 h to form a uniform electrospinning solution.
[0065] (2) The electrospinning solution obtained in step (1) was transferred to a plastic syringe with a 21 G needle for electrospinning. The spinning distance between the syringe needle and the collector was 15 cm, the spinning voltage was 14 kV, the spinning speed was 1 mL / h, and the air humidity was 40%, thereby obtaining nanofibers.
[0066] (3) The nanofibers obtained in step (2) were pre-oxidized, heated to 220 °C in a muffle furnace at a rate of 1 °C / min and kept warm for 2 h; 500 mg of selenium powder was placed upstream of the tube furnace, and 150 mg of the pre-oxidized nanofibers were placed downstream of the tube furnace, first heated to 550 °C at a rate of 2 °C / min and kept warm for 1 h, and then heated to 900 °C at a rate of 5 °C / min and kept warm for 2 h, to obtain NiSe@CNF, a self-supporting positive electrode material for lithium-sulfur batteries. Comparative Example 2
[0067] A method for preparing a self-supporting positive electrode material for a lithium-sulfur battery comprises the following steps:
[0068] (1) 1000 mg of polyacrylonitrile, 0.72 mmol Ni(CH3COO)2·4H2O and 0.08 mmol Eu(C2H3O2)3·4H2O were dissolved in 10 mL N,N-dimethylformamide (DMF) (the molar ratio of Ni(CH3COO)2·4H2O to Eu(C2H3O2)3·4H2O was 9:1) and stirred in an oil bath at 60 °C for 12 h to form a uniform electrospinning solution.
[0069] (2) The electrospinning solution obtained in step (1) was transferred to a plastic syringe with a 21 G needle for electrospinning. The spinning distance between the syringe needle and the collector was 15 cm, the spinning voltage was 14 kV, the spinning speed was 1 mL / h, and the air humidity was 40%, thereby obtaining nanofibers.
[0070] (3) The nanofibers obtained in step (2) are pre-oxidized, heated to 220°C at a rate of 1°C / min in a muffle furnace and kept warm for 2 h; 500 mg of selenium powder is placed upstream of the tube furnace, and 150 mg of the pre-oxidized nanofibers are placed downstream of the tube furnace, first heated to 550°C at a rate of 2°C / min and kept warm for 1 h, and then heated to 900°C at a rate of 5°C / min and kept warm for 2 h, to obtain a self-supporting positive electrode material for a lithium-sulfur battery.
[0071] The NiSe-Eu@CNF prepared in Example 1 and the NiSe@CNF prepared in Comparative Example 1 were characterized in terms of morphology. Figure 1 and Figure 2As shown. In the present invention, metal salts are added during the preparation of the electrospinning solution, so during the high-temperature calcination process, the organic polyacrylonitrile will form carbon nanofibers, and the metal salt will precipitate at high temperature to form selenide nanoparticles in a selenized atmosphere, thereby obtaining nanoparticles loaded with carbon nanofibers, and the specific microscopic morphology is shown as follows Figure 1 As shown in (a). Figure 2 In (c), we can see the lattice fringes of NiSe. Figure 1 In (c), it can be seen that the lattice spacing of NiSe is enlarged, indicating that Eu is doped into the NiSe lattice. Considering that the radius of Eu atoms is large, it is unlikely to exist in interstitial sites. In addition, the high-resolution lattice spacing is not enlarged much. It is speculated that this doping is to replace the Ni metal sites in NiSe.
[0072] The elemental composition of NiSe-Eu@CNF prepared in Example 1 was tested, and the test results of X-ray energy spectrum elemental imaging analysis technology (EDS mapping) are as follows: Figure 3 As shown, from Figure 3 Eu doping can also be seen in the MgO2O3.
[0073] The crystal structures of the NiSe-Eu@CNF prepared in Example 1, the NiSe@CNF prepared in Comparative Example 1 and the self-supporting positive electrode materials for lithium-sulfur batteries prepared in Comparative Example 2 were tested by X-ray diffraction (XRD). The test results are as follows: Figure 4 and Figure 5 As shown, from Figure 4 It can be seen that the doping of Eu does not affect the crystal structure of NiSe; Figure 5 It can be seen that the doping of Eu should be small. Excessive doping will lead to Eu agglomeration, and uniform Eu-doped NiSe material cannot be prepared. Instead, EuSe phase will appear, and the positive electrode material may become a NiSe / EuSe heterojunction. The action mechanism of the heterojunction is different from that of the doped material, and the catalytic activity of the metal active sites and the non-metal active sites cannot be activated at the same time.
[0074] Test Example 1
[0075] The adsorption capacity of NiSe-Eu@CNF prepared in Example 1 and NiSe@CNF prepared in Comparative Example 1 for Li2S6 was tested.
[0076] The testing method is as follows: grind the NiSe-Eu@CNF prepared in Example 1 and the NiSe@CNF prepared in Comparative Example 1 into powder, take 20 mg of the powder and add it into 3 mL of 0.75 mM Li2S6 solution, observe the color of the solution after standing and adsorbing for 2 hours, and test the ultraviolet visible light (UV-Vis) spectrum; use the synchrotron radiation X-ray absorption spectrum of the Shanghai Light Source BL11B test line station to test the K-edge absorption spectra of Ni and Se of NiSe-Eu@CNF and NiSe@CNF before and after the adsorption of Li2S6.
[0077] Test results such as Figure 6 and Figure 7 As shown, from Figure 6 As can be seen in (a), the color of the Li2S6 solution after adsorption by NiSe-Eu@CNF is lighter at the same time, indicating that the adsorption effect of NiSe-Eu@CNF is better. Figure 6 It can also be seen in (b) that the intensity of the characteristic peak of Li2S6 molecules after adsorption by NiSe-Eu@CNF is lower, proving that NiSe-Eu@CNF has a better effect in adsorbing Li2S6 than NiSe@CNF. Figure 7 It can be seen that the movement of the absorption edge reflects whether the element participates in the adsorption process of Li2S6. Obviously, for NiSe@CNF, the absorption edge of Ni has a small movement, while the absorption edge of Se has almost no change. In NiSe-Eu@CNF, the K edges of Ni and Se have changed significantly, indicating that Eu doping enhances the activity of both Ni and Eu.
[0078] Test Example 2
[0079] The lithium-sulfur battery self-supporting positive electrode material NiSe-Eu@CNF prepared in Example 1 and the lithium-sulfur battery self-supporting positive electrode material NiSe@CNF prepared in Comparative Example 1 were used to assemble a lithium-sulfur battery. The assembly method was as follows: the lithium-sulfur battery self-supporting positive electrode material was cut into a positive electrode sheet with a diameter of 12 mm by a slicer, the metal lithium was used as the negative electrode sheet, the positive electrode sheet was bonded to the Celgard 2500 separator, and the other side of the separator was bonded to the negative electrode sheet. The positive electrode sheet, separator and negative electrode sheet bonded into one were placed in a lithium-sulfur battery housing, 12.5 μL of 0.5 M Li2S6 solution and 17.5 μL of LiTFSI with a concentration of 5 mol·L were added dropwise. -1 The ether electrolyte is prepared by dissolving LiTFSI in a mixed solution of DME and DOL with a volume ratio of 1:1, and the lithium-sulfur battery is assembled after sealing.
[0080] The cycling performance of the lithium-sulfur battery assembled with NiSe-Eu@CNF prepared in Example 1 and NiSe@CNF prepared in Comparative Example 1 was tested. Figure 8 , Fig. 9 , Fig.10 and Fig.11 As shown, Figure 8 This is a cycling performance diagram of a lithium-sulfur battery assembled with NiSe-Eu@CNF prepared in Example 1 and NiSe@CNF prepared in Comparative Example 1 at 0.2 C. Fig. 9 The rate performance diagram of the lithium-sulfur battery assembled with NiSe-Eu@CNF prepared in Example 1 shows that 896.2 mAh·g -1 High discharge capacity. Fig.10 This is the long cycle performance diagram of the lithium-sulfur battery assembled with NiSe-Eu@CNF prepared in Example 1 at 1C. After 500 cycles, the lithium-sulfur battery still has 657.8 mAh·g -1 The discharge specific capacity of the battery is only 0.08% per cycle.
[0081] Fig.11 The sulfur loading of NiSe-Eu@CNF prepared in Example 1 is 5.94 mg·cm -2 The cycling performance of the lithium-sulfur battery at a current density of 0.05 C. The sulfur loading is obtained by dividing the mass of sulfur in the active material by the area of the positive electrode. When the sulfur loading reaches 5.94 mg cm -2 The assembled lithium-sulfur battery can still obtain 5.68 mAh·cm -2 The high reversible capacity can be stably cycled 100 times.
[0082] In summary, the self-supporting positive electrode material NiSe-Eu@CNF for lithium-sulfur batteries prepared by the present invention improves the capacity and energy density of lithium-sulfur batteries by combining a self-supporting carbon positive electrode with a nano-metal catalyst. On this basis, the introduction of metal Eu simultaneously activates the catalytic activity of the metal active site Ni and the non-metal active site Se, improves the performance of metal Ni as a catalytic active substance, and achieves better rate performance and cycle stability. In addition, this technical solution realizes high-load cycling of lithium-sulfur batteries at room temperature, and has potential practical commercial application value.
[0083] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a self-supporting positive electrode material for a lithium-sulfur battery, characterized in that: The following steps are involved: (1) dissolving polyacrylonitrile, nickel salt and europium salt in N,N-dimethylformamide, stirring evenly to obtain an electrospinning solution, wherein the molar ratio of the nickel salt to the europium salt is (10-20):1; (2) electrospinning the electrospinning solution obtained in step (1) to obtain nanofibers; (3) The nanofibers obtained in step (2) are subjected to a pre-oxidation treatment, and the pre-oxidation nanofibers are subjected to a carbonization treatment in a selenium vapor atmosphere to obtain the self-supporting positive electrode material for a lithium-sulfur battery.
2. The preparation method according to claim 1, characterized in that: In step (1), the concentration of polyacrylonitrile in the electrospinning solution is 50-200 mg / mL, and the sum of the concentrations of nickel salt and europium salt in the electrospinning solution is 40-80 mM.
3. The preparation method according to claim 1, characterized in that: In step (1), the nickel salt is selected from one or more of nickel nitrate, nickel chloride and nickel sulfate, and the europium salt is europium chloride and / or europium acetate.
4. The preparation method according to claim 1, characterized in that: In step (2), the electrospinning conditions are: spinning distance is 13-18 cm, spinning voltage is 13-15 kV, and spinning speed is 0.8-1.1 mL / h.
5. The preparation method according to claim 1, characterized in that: In step (3), the pre-oxidation treatment is specifically as follows: placing the nanofibers in a heating device, heating the temperature to 210-230°C at a rate of 1-3°C / min, and keeping the temperature for 2-4 hours.
6. The preparation method according to claim 1, characterized in that: In step (3), the carbonization treatment is carried out in a tubular furnace, the selenium powder is placed upstream of the tubular furnace, and the nanofibers after the pre-oxidation treatment are placed downstream of the tubular furnace.
7. The preparation method according to claim 6, characterized in that: The mass ratio of the selenium powder to the pre-oxidized nanofibers is (3-20):
1.
8. The preparation method according to claim 1, characterized in that: In step (3), the carbonization treatment is specifically as follows: firstly, the temperature is raised to 500-600°C at a rate of 1-3°C / min and kept at that temperature for 1-2 h, and then the temperature is raised to 800-1000°C at a rate of 5-7°C / min and kept at that temperature for 2-4 h.
9. A self-supporting positive electrode material for a lithium-sulfur battery prepared by the method according to any one of claims 1 to 8.
10. A lithium-sulfur battery, characterized in that: Including the self-supporting positive electrode material for lithium-sulfur batteries as described in claim 9.