A safe and environmentally friendly sizing agent for papermaking and preparation method thereof

By using a two-layer sizing agent prepared by organic boric acid-modified polyvinylamine and modified polyvinyl alcohol in the papermaking process, the problem of insufficient performance improvement of existing sizing agents is solved, and the mechanical strength and water resistance of paper are achieved. Significant improvement, especially the improvement of tensile wet strength and ink adhesion.

CN118531656BActive Publication Date: 2024-10-18NANTONG TENGLONG CHEM TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411005275.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-18
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Existing papermaking sizing agents have shortcomings in improving paper properties, especially low water resistance, folding endurance and ring crush strength.

Method used

A sizing agent prepared from organic boric acid-modified polyvinylamine and modified polyvinyl alcohol is used to enhance the mechanical strength and water resistance of the paper through a two-layer coating structure (glue layer A and glue layer B), and carboxyl silane is used to assist Agent improves ink adhesion.

Benefits of technology

Significantly improves the paper's folding endurance, tensile strength, tensile wet strength, bursting strength and ink adhesion, forming a multiple cross-linked network structure to enhance paper density and water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118531656B_ABST
    Figure CN118531656B_ABST
Patent Text Reader

Abstract

The invention relates to the field of papermaking chemicals, and in particular to a safe and environmentally friendly sizing agent for papermaking and a preparation method thereof. The sizing agent comprises a glue layer A and a glue layer B which are sequentially coated on the surface of paper, wherein the glue layer A is obtained by coating a glue solution A on the surface of paper, and the glue layer B is obtained by coating the glue solution B on the surface of the glue layer A, wherein the mass ratio of the glue solution A to the glue solution B is 0.2-0.25:2.5-3, the glue solution A is prepared by organic boron-modified polyvinyl amine, and the glue solution B comprises the following raw materials in parts by mass: 35-45 parts of a base polyvinyl alcohol solution, 4.9-5.15 parts of a modified polyvinyl alcohol A, 4.9-5.15 parts of a modified polyvinyl alcohol B, and 3-3.25 parts of an auxiliary agent. The invention discloses a sizing agent for reinforcing paper by compounding the sizing solution A and the sizing solution B as a sizing agent, so that the prepared paper with the sizing agent coated on the surface has strong folding endurance, tensile strength, tensile wet strength, water resistance and ink adhesion, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of papermaking chemicals, and in particular to a safe and environmentally friendly sizing agent for papermaking and a preparation method thereof. Background Art

[0002] Paper is considered to be the most economical and environmentally friendly material. The application of papermaking chemicals plays a decisive role in the quality of paper and the operation of production. Papermaking chemicals give paper various excellent special properties, such as water resistance, oil resistance, wet strength, oxygen barrier, smoothness and softness. Papermaking chemicals refer to the general term for various chemical agents and additives used in the papermaking process, including sizing agents, wet strength agents, etc.

[0003] The commonly used surface sizing agent in the prior art is starch. For example, the invention patent with publication number CN108824079A discloses a rice starch sizing agent. The invention improves the surface strength of paper by treating rice starch. However, the starch sizing agent is easy to absorb moisture after film formation, which affects the water resistance of paper, and has low bursting resistance and ring crush strength. In addition to starch, alkyl ketene dimer (AKD) is also a good reactive sizing agent because it has good water resistance. For example, the invention patent with publication number CN114539190B discloses a preparation method of alkyl ketene dimer. Although the invention can effectively avoid the adverse effects such as the decrease in the sizing effect of alkyl ketene dimer caused by the auxiliary component, the alkyl ketene dimer has poor affinity with paper fibers and is not very helpful in improving the ring crush strength and stiffness of paper.

[0004] Therefore, according to the above-mentioned related technologies, it is urgent to develop a safe and environmentally friendly papermaking sizing agent and a preparation method thereof. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a safe and environmentally friendly sizing agent for papermaking and a preparation method thereof, so as to solve the problem that the sizing agent in the prior art has poor improvement on the performance of paper.

[0006] Based on the above purpose, the present invention provides a safe and environmentally friendly sizing agent for papermaking and a preparation method thereof.

[0007] A safe and environmentally friendly sizing agent for papermaking, the sizing agent comprising a glue layer A and a glue layer B sequentially coated on the surface of paper;

[0008] The glue layer A is obtained by coating glue liquid A on the surface of paper, and the glue layer B is obtained by coating glue liquid B on the surface of the glue layer A, and the mass ratio of the glue liquid A to the glue liquid B is 0.2-0.25:2.5-3;

[0009] The glue A is prepared by modifying polyvinyl amine with organic boric acid;

[0010] The glue solution B comprises the following raw materials in parts by weight: 35-45 parts of base polyvinyl alcohol solution, 4.9-5.15 parts of modified polyvinyl alcohol A, 4.9-5.15 parts of modified polyvinyl alcohol B, and 3-3.25 parts of additives;

[0011] The concentration of the matrix polyvinyl alcohol solution is 8%-10%;

[0012] The modified polyvinyl alcohol A is polyvinyl alcohol modified by a silane coupling agent;

[0013] The modified polyvinyl alcohol B is isocyanate-modified polyvinyl alcohol;

[0014] The auxiliary agent is carboxyl silane.

[0015] Preferably, the preparation method of the modified polyvinyl alcohol A is as follows:

[0016] Add polyvinyl alcohol to deionized water, stir at 85-90°C for 1.5-2h to obtain a polyvinyl alcohol solution, then cool to 55-60°C, add KH-560 dropwise, and adjust the pH value of the reaction system to 7-8 with 10% sodium hydroxide solution, then stir at 190-200r / min for 1.5-2h to obtain modified polyvinyl alcohol A.

[0017] Preferably, the concentration of the polyvinyl alcohol solution is 8%-10%, and the mass ratio of the polyvinyl alcohol solution to KH-560 is 8-9:1.25-1.5.

[0018] Preferably, the preparation method of the modified polyvinyl alcohol B is as follows:

[0019] Step A1. Add polyvinyl alcohol to toluene and stir at 85-90° C. for 3.5-4 h to obtain a polyvinyl alcohol solution;

[0020] Step A2. Mix butanone oxime and isophorone diisocyanate, add dibutyltin dilaurate, stir at a temperature of 55-60°C and a stirring speed of 180-200 r / min for 2.5-3h, then cool to 35-40°C, add the polyvinyl alcohol solution prepared in step A1, react for 25-30min, and obtain modified polyvinyl alcohol B.

[0021] Preferably, the concentration of the polyvinyl alcohol solution in step A1 is 16%-18%.

[0022] Preferably, in step A2, the molar ratio of butanone oxime to isophorone diisocyanate is 1.5-2:0.9-1.15, and the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 8-10:1.5-2.

[0023] Preferably, the preparation method of the carboxyl-terminated polysiloxane is as follows:

[0024] Step B1. react octamethylcyclotetrasiloxane, KH-551, methyldimethoxydodecylsilane, tetramethylammonium hydroxide and 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane in an oil bath at 90-100°C for 5.5-6h, then raise the system temperature to 135-140°C, maintain reflux for 40-60min, remove low boiling points under reduced pressure, and obtain amino silicone oil;

[0025] Step B2. Mix amino silicone oil and maleic anhydride, heat to 65-70° C., and react for 40-60 min to obtain carboxyl silane.

[0026] Preferably, the mass ratio of octamethylcyclotetrasiloxane, KH-551, methyldimethoxydodecylsilane, tetramethylammonium hydroxide and 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane in step B1 is 25-30:1.75-2:9-11:0.045-0.05:26-28.

[0027] Preferably, the molar ratio of amino group to maleic anhydride in the amino silicone oil in step B2 is 1:1-1.05.

[0028] A safe and environmentally friendly sizing agent for papermaking, the preparation method of the sizing agent is as follows:

[0029] Step S1. dissolving the organic boric acid modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.01wt%-0.015wt%, immersing the paper in the aqueous solution for 8-10 minutes, then washing the paper with a 2mM NaCl deionized water solution, and then drying the paper at 25-30°C for 5-7 minutes to obtain sizing solution A sizing paper;

[0030] Step S2. The base polyvinyl alcohol solution, modified polyvinyl alcohol A, modified polyvinyl alcohol B and the additive are mixed evenly, and heated at 85-90° C. for 1-2 h to obtain glue solution B;

[0031] Step S3. Fix the sizing liquid A coated paper and use a coating machine to apply sizing liquid B at a sizing rate of 3.0-4.0 mm / s to apply sizing to the surface. Put the sizing paper into a constant temperature box and dry it at a temperature of 50-60° C. for 13-15 minutes to obtain the sizing agent coated on the surface of the paper.

[0032] Beneficial effects of the present invention:

[0033] The present invention provides a safe and environmentally friendly sizing agent for papermaking and a preparation method thereof. The sizing agent provided by the present invention can improve the folding endurance, tensile strength, tensile wet strength, bursting resistance, water resistance and ink adhesion of paper, and has broad application prospects compared with the prior art.

[0034] The present invention provides a safe and environmentally friendly sizing agent for papermaking and a preparation method thereof. The sizing solution A provided by the present invention can simultaneously form a bonding effect with the sizing solution B and paper to form a multiple cross-linked network structure inside the system. On the one hand, the density of the paper can be increased by filling the pores in the paper fibers, thereby increasing the strength of the paper. On the other hand, the water resistance of the paper can be increased by blocking water. In addition, by introducing carboxyl groups inside the system, ink particles are easily dispersed and can then penetrate into the paper fibers and be anchored in the small gaps inside the network structure, thereby enhancing the adhesion of the paper to the ink. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 This is a schematic diagram of the sized paper with the sizing agent coated on the surface prepared in Example 1 of the present invention;

[0037] Figure 2 This is a schematic diagram of the sized paper with sizing agent coated on the surface prepared in Comparative Example 5 of the present invention. DETAILED DESCRIPTION

[0038] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0039] The polyvinyl alcohol used in the present invention was purchased from Shanghai Yingjia Industrial Development Co., Ltd., with a model of PVA1799 and a degree of alcoholysis of 99%.

[0040] Embodiment 1: A method for preparing a safe and environmentally friendly papermaking sizing agent, comprising the following steps:

[0041] Step S1. Add polyvinyl alcohol to deionized water, stir at 85°C for 1.5h to obtain a polyvinyl alcohol solution with a concentration of 8%, then cool to 55°C, drop 1.25g KH-560 into 8g of the polyvinyl alcohol solution, and adjust the pH value of the reaction system to 7 with 10% sodium hydroxide solution, and then stir at a speed of 190r / min for 1.5h to obtain modified polyvinyl alcohol A;

[0042] Step S2. adding polyvinyl alcohol to toluene and stirring at 85° C. for 3.5 h to obtain a polyvinyl alcohol solution with a concentration of 16%;

[0043] Step S3. Mix butanone oxime and isophorone diisocyanate, wherein the molar ratio of butanone oxime to isophorone diisocyanate is 1.5:0.9, add dibutyltin dilaurate, stir for 2.5 hours at a temperature of 55° C. and a stirring speed of 180 r / min, then cool to 35° C., add the polyvinyl alcohol solution prepared in step S2, wherein the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 8:1.5, react for 25 minutes, and obtain modified polyvinyl alcohol B;

[0044] Step S4. 25 g of octamethylcyclotetrasiloxane, 1.75 g of KH-551, 9 g of methyldimethoxydodecylsilane, 0.045 g of tetramethylammonium hydroxide and 26 g of 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane were reacted in an oil bath at 90° C. for 5.5 h, and then the system temperature was raised to 135° C. and kept at reflux for 40 min. Low boiling substances were removed under reduced pressure to obtain amino silicone oil;

[0045] Step S5. Mixing amino silicone oil and maleic anhydride in a molar ratio of 1:1 between the amino group in the amino silicone oil and the maleic anhydride, heating to 65° C., and reacting for 40 min to obtain an auxiliary agent;

[0046] Step S6. dissolving the organic boric acid-modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.01 wt%, immersing the paper in the aqueous solution for 8 min, then washing the paper with a 2 mM NaCl deionized aqueous solution, and then drying the paper at 25° C. for 5 min to obtain sizing solution A sized paper;

[0047] Step S7. 35 g of the base polyvinyl alcohol solution, 4.9 g of modified polyvinyl alcohol A, 4.9 g of modified polyvinyl alcohol B and 3 g of the additive were mixed evenly, and heated at 85° C. for 1 h to obtain glue solution B;

[0048] Step S8. After fixing the sizing liquid A coated paper, use a coating machine to apply sizing liquid B at a sizing rate of 3.0 mm / s, wherein the mass ratio of sizing liquid A to sizing liquid B is 0.2:2.5, and the sizing paper is placed in a constant temperature box and dried at a temperature of 50°C for 13 minutes to obtain the sizing agent coated on the surface of the paper.

[0049] Embodiment 2: A method for preparing a safe and environmentally friendly papermaking sizing agent, comprising the following steps:

[0050] Step S1. Add polyvinyl alcohol to deionized water, stir at 86°C for 1.6 hours to obtain a polyvinyl alcohol solution with a concentration of 9%, then cool to 56°C, drop 1.3g KH-560 into 8.2g of the polyvinyl alcohol solution, and adjust the pH value of the reaction system to 7.5 with 10% sodium hydroxide solution, and then stir at a speed of 192r / min for 1.6 hours to obtain modified polyvinyl alcohol A;

[0051] Step S2. adding polyvinyl alcohol to toluene, stirring at 86° C. for 3.6 h to obtain a polyvinyl alcohol solution with a concentration of 17%;

[0052] Step S3. Mix butanone oxime and isophorone diisocyanate, wherein the molar ratio of butanone oxime to isophorone diisocyanate is 1.6:0.95, add dibutyltin dilaurate, stir for 2.6 hours at a temperature of 56° C. and a stirring speed of 184 r / min, then cool to 36° C., add the polyvinyl alcohol solution prepared in step S2, wherein the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 9:1.6, react for 26 minutes, and obtain modified polyvinyl alcohol B;

[0053] Step S4. 26 g of octamethylcyclotetrasiloxane, 1.8 g of KH-551, 9.4 g of methyldimethoxydodecylsilane, 0.046 g of tetramethylammonium hydroxide and 26.4 g of 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane were reacted in an oil bath at 92° C. for 5.6 h, and then the system temperature was raised to 136° C. and kept at reflux for 44 min. Low-boiling substances were removed under reduced pressure to obtain amino silicone oil;

[0054] Step S5. amino silicone oil and maleic anhydride are mixed according to a molar ratio of amino group in the amino silicone oil to maleic anhydride of 1:1.01, heated to 66° C., and reacted for 44 minutes to obtain an auxiliary agent;

[0055] Step S6. dissolving the organic boric acid-modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.011 wt%, immersing the paper in the aqueous solution for 9 minutes, then washing the paper with a 2 mM NaCl deionized water solution, and then drying the paper at 26° C. for 6 minutes to obtain sizing solution A sizing paper;

[0056] Step S7. 37 g of the base polyvinyl alcohol solution, 4.95 g of modified polyvinyl alcohol A, 4.95 g of modified polyvinyl alcohol B and 3.05 g of the additive were mixed evenly, and heated at 86° C. for 1.5 h to obtain glue solution B;

[0057] Step S8. After fixing the sizing liquid A coated paper, use a coating machine to apply sizing liquid B at a sizing rate of 3.2 mm / s, wherein the mass ratio of sizing liquid A to sizing liquid B is 0.21:2.6, and the sizing paper is placed in a constant temperature box and dried at a temperature of 52° C. for 14 minutes to obtain the sizing agent coated on the surface of the paper.

[0058] Embodiment 3: A method for preparing a safe and environmentally friendly papermaking sizing agent, comprising the following steps:

[0059] Step S1. Add polyvinyl alcohol to deionized water, stir at 87°C for 1.7h to obtain a polyvinyl alcohol solution with a concentration of 10%, then cool to 57°C, drop 1.35g KH-560 into 8.4g polyvinyl alcohol solution, adjust the pH value of the reaction system to 8 with 10% sodium hydroxide solution, and stir at a speed of 194r / min for 1.7h to obtain modified polyvinyl alcohol A;

[0060] Step S2. adding polyvinyl alcohol to toluene and stirring at 87° C. for 3.7 h to obtain a polyvinyl alcohol solution with a concentration of 18%;

[0061] Step S3. Mix butanone oxime and isophorone diisocyanate, wherein the molar ratio of butanone oxime to isophorone diisocyanate is 1.7:1, add dibutyltin dilaurate, stir at a temperature of 57° C. and a stirring speed of 188 r / min for 2.7 h, then cool to 37° C., add the polyvinyl alcohol solution prepared in step S2, wherein the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 10:1.7, react for 27 min, and obtain modified polyvinyl alcohol B;

[0062] Step S4. 27 g of octamethylcyclotetrasiloxane, 1.85 g of KH-551, 9.8 g of methyldimethoxydodecylsilane, 0.047 g of tetramethylammonium hydroxide and 26.8 g of 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane were reacted in an oil bath at 94 ° C for 5.7 h, and then the system temperature was raised to 137 ° C, maintained at reflux for 48 min, and low-boiling substances were removed under reduced pressure to obtain amino silicone oil;

[0063] Step S5. amino silicone oil and maleic anhydride are mixed according to a molar ratio of amino group in the amino silicone oil to maleic anhydride of 1:1.02, heated to 67° C., and reacted for 48 minutes to obtain an auxiliary agent;

[0064] Step S6. dissolving the organic boric acid-modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.012 wt %, immersing the paper in the aqueous solution for 10 min, then washing the paper with a 2 mM NaCl deionized water solution, and then drying the paper at 27° C. for 7 min to obtain sizing solution A sized paper;

[0065] Step S7. 39 g of the base polyvinyl alcohol solution, 5 g of modified polyvinyl alcohol A, 5 g of modified polyvinyl alcohol B and 3.15 g of the additive were mixed evenly, and heated at 87° C. for 2 h to obtain glue solution B;

[0066] Step S8. After fixing the sizing liquid A coated paper, use a coating machine to apply sizing liquid B at a sizing rate of 3.4 mm / s, wherein the mass ratio of sizing liquid A to sizing liquid B is 0.22:2.7, and the sizing paper is placed in a constant temperature box and dried at a temperature of 5.4°C for 15 minutes to obtain the sizing agent coated on the surface of the paper.

[0067] Embodiment 4: A method for preparing a safe and environmentally friendly papermaking sizing agent, comprising the following steps:

[0068] Step S1. Add polyvinyl alcohol to deionized water, stir at 88°C for 1.8h to obtain a polyvinyl alcohol solution with a concentration of 8%, then cool to 58°C, drop 1.4g KH-560 into 8.6g polyvinyl alcohol solution, adjust the pH value of the reaction system to 7 with 10% sodium hydroxide solution, and stir at a speed of 196r / min for 1.8h to obtain modified polyvinyl alcohol A;

[0069] Step S2. adding polyvinyl alcohol to toluene and stirring at 88° C. for 3.8 h to obtain a polyvinyl alcohol solution with a concentration of 16%;

[0070] Step S3. Mix butanone oxime and isophorone diisocyanate, wherein the molar ratio of butanone oxime to isophorone diisocyanate is 1.8:1.05, add dibutyltin dilaurate, stir for 2.8 hours at a temperature of 58° C. and a stirring speed of 192 r / min, then cool to 38° C., add the polyvinyl alcohol solution prepared in step S2, wherein the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 8:1.8, react for 28 minutes, and obtain modified polyvinyl alcohol B;

[0071] Step S4. 28 g of octamethylcyclotetrasiloxane, 1.9 g of KH-551, 10.2 g of methyldimethoxydodecylsilane, 0.048 g of tetramethylammonium hydroxide and 27.2 g of 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane were reacted in an oil bath at 96 ° C for 5.8 h, and then the system temperature was raised to 138 ° C, maintained at reflux for 52 min, and low-boiling substances were removed under reduced pressure to obtain amino silicone oil;

[0072] Step S5. amino silicone oil and maleic anhydride are mixed according to a molar ratio of amino group in the amino silicone oil to maleic anhydride of 1:1.03, heated to 68° C., and reacted for 52 minutes to obtain an auxiliary agent;

[0073] Step S6. dissolving the organic boric acid-modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.013 wt %, immersing the paper in the aqueous solution for 8 min, then washing the paper with a 2 mM NaCl deionized aqueous solution, and then drying the paper at 28° C. for 5 min to obtain sizing solution A sizing paper;

[0074] Step S7. 41 g of the base polyvinyl alcohol solution, 5.05 g of modified polyvinyl alcohol A, 5.05 g of modified polyvinyl alcohol B and 3.15 g of the additive were mixed evenly, and heated at 88° C. for 1 h to obtain glue solution B;

[0075] Step S8. After fixing the sized paper with sizing liquid A, use a coating machine to apply sizing liquid B at a sizing rate of 3.6 mm / s, wherein the mass ratio of sizing liquid A to sizing liquid B is 0.23:2.8, and the sizing paper is placed in a constant temperature box and dried at a temperature of 56°C for 13 minutes to obtain the sizing agent coated on the surface of the paper.

[0076] Embodiment 5: A method for preparing a safe and environmentally friendly papermaking sizing agent, comprising the following steps:

[0077] Step S1. Add polyvinyl alcohol to deionized water, stir at 89° C. for 1.9 h to obtain a polyvinyl alcohol solution with a concentration of 9%, then cool to 59° C., drop 1.45 g KH-560 into 8.8 g of the polyvinyl alcohol solution, and adjust the pH value of the reaction system to 7.5 with 10% sodium hydroxide solution, and then stir at a speed of 198 r / min for 1.9 h to obtain modified polyvinyl alcohol A;

[0078] Step S2. adding polyvinyl alcohol to toluene, stirring at 89° C. for 3.9 h to obtain a polyvinyl alcohol solution with a concentration of 17%;

[0079] Step S3. Mix butanone oxime and isophorone diisocyanate, wherein the molar ratio of butanone oxime to isophorone diisocyanate is 1.9:1.1, add dibutyltin dilaurate, stir for 2.9 hours at a temperature of 59° C. and a stirring speed of 196 r / min, then cool to 39° C., add the polyvinyl alcohol solution prepared in step S2, wherein the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 9:1.9, react for 29 minutes, and obtain modified polyvinyl alcohol B;

[0080] Step S4. 29 g of octamethylcyclotetrasiloxane, 1.95 g of KH-551, 10.6 g of methyldimethoxydodecylsilane, 0.049 g of tetramethylammonium hydroxide and 27.6 g of 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane were reacted in an oil bath at 98 ° C for 5.9 h, and then the system temperature was raised to 139 ° C, maintained at reflux for 56 min, and low-boiling substances were removed under reduced pressure to obtain amino silicone oil;

[0081] Step S5. amino silicone oil and maleic anhydride are mixed according to a molar ratio of amino group in the amino silicone oil to maleic anhydride of 1:1.04, heated to 69° C., and reacted for 56 minutes to obtain an auxiliary agent;

[0082] Step S6. dissolving the organic boric acid-modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.014 wt%, immersing the paper in the aqueous solution for 9 minutes, then washing the paper with a 2 mM NaCl deionized water solution, and then drying the paper at 29° C. for 6 minutes to obtain sizing solution A sized paper;

[0083] Step S7. 43 g of the base polyvinyl alcohol solution, 5.1 g of modified polyvinyl alcohol A, 5.1 g of modified polyvinyl alcohol B and 3.2 g of the additive were mixed evenly, and heated at 89° C. for 1.5 h to obtain glue solution B;

[0084] Step S8. After fixing the sizing liquid A coated paper, use a coating machine to apply sizing liquid B at a sizing rate of 3.8 mm / s, wherein the mass ratio of sizing liquid A to sizing liquid B is 0.24:2.9, and the sizing paper is placed in a constant temperature box and dried at a temperature of 58°C for 14 minutes to obtain the sizing agent coated on the surface of the paper.

[0085] Embodiment 6: A method for preparing a safe and environmentally friendly papermaking sizing agent, comprising the following steps:

[0086] Step S1. Add polyvinyl alcohol to deionized water, stir at 90°C for 2h to obtain a polyvinyl alcohol solution with a concentration of 10%, then cool to 60°C, drop 1.5g KH-560 into 9g of the polyvinyl alcohol solution, and adjust the pH value of the reaction system to 8 with 10% sodium hydroxide solution, and then stir at a speed of 200r / min for 2h to obtain modified polyvinyl alcohol A;

[0087] Step S2. adding polyvinyl alcohol to toluene and stirring at 90° C. for 4 h to obtain a polyvinyl alcohol solution with a concentration of 18%;

[0088] Step S3. Mix butanone oxime and isophorone diisocyanate, wherein the molar ratio of butanone oxime to isophorone diisocyanate is 2:1.15, add dibutyltin dilaurate, stir at a temperature of 60°C and a stirring speed of 200 r / min for 3 hours, then cool to 40°C, add the polyvinyl alcohol solution prepared in step S2, wherein the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 10:2, and react for 30 minutes to obtain modified polyvinyl alcohol B;

[0089] Step S4. 30 g of octamethylcyclotetrasiloxane, 2 g of KH-551, 11 g of methyldimethoxydodecylsilane, 0.05 g of tetramethylammonium hydroxide and 28 g of 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane were reacted in an oil bath at 100 ° C for 6 h, and then the system temperature was raised to 140 ° C, maintained at reflux for 60 min, and low-boiling substances were removed under reduced pressure to obtain amino silicone oil;

[0090] Step S5. amino silicone oil and maleic anhydride are mixed according to a molar ratio of amino group in the amino silicone oil to maleic anhydride of 1:1.05, heated to 70° C., and reacted for 60 min to obtain an auxiliary agent;

[0091] Step S6. dissolving the organic boric acid modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.015 wt %, immersing the paper in the aqueous solution for 10 min, then washing the paper with a 2 mM NaCl deionized water solution, and then drying the paper at 30° C. for 7 min to obtain sizing solution A sized paper;

[0092] Step S7. 45 g of the base polyvinyl alcohol solution, 5.15 g of modified polyvinyl alcohol A, 5.15 g of modified polyvinyl alcohol B and 3.25 g of the additive were mixed evenly, and heated at 90° C. for 2 h to obtain glue solution B;

[0093] Step S8. After fixing the sizing liquid A coated paper, use a coating machine to apply sizing liquid B at a sizing rate of 4.0 mm / s, wherein the mass ratio of sizing liquid A to sizing liquid B is 0.25:3, and the sizing paper is placed in a constant temperature box and dried at a temperature of 60°C for 15 minutes to obtain the sizing agent coated on the surface of the paper.

[0094] Comparative Example 1:

[0095] Compared with Example 1, the sizing liquid A was not added during the preparation of the sizing agent in this comparative example, and the remaining steps and parameters were the same, which will not be repeated in this comparative example. Finally, a sizing agent coated on the surface of paper was obtained.

[0096] Comparative Example 2:

[0097] Compared with Example 1, this comparative example only adjusts the mass ratio of sizing solution A to sizing solution from "0.2:2.5" to "2.5:0.2", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a sizing agent coated on the surface of paper is obtained.

[0098] Comparative Example 3:

[0099] Compared with Example 1, this comparative example only replaces "modified polyvinyl alcohol A" with "modified polyvinyl alcohol B", and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, a sizing agent coated on the surface of paper is obtained.

[0100] Comparative Example 4:

[0101] Compared with Example 1, this comparative example only replaces "modified polyvinyl alcohol B" with "modified polyvinyl alcohol A", and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, a sizing agent coated on the surface of paper is obtained.

[0102] Comparative Example 5:

[0103] Step S1. Add polyvinyl alcohol to deionized water, stir at 85°C for 1.5h to obtain a polyvinyl alcohol solution with a concentration of 8%, then cool to 55°C, drop 1.25g KH-560 into 8g of the polyvinyl alcohol solution, and adjust the pH value of the reaction system to 7 with 10% sodium hydroxide solution, and then stir at a speed of 190r / min for 1.5h to obtain modified polyvinyl alcohol A;

[0104] Step S2. adding polyvinyl alcohol to toluene and stirring at 85° C. for 3.5 h to obtain a polyvinyl alcohol solution with a concentration of 16%;

[0105] Step S3. Mix butanone oxime and isophorone diisocyanate, wherein the molar ratio of butanone oxime to isophorone diisocyanate is 1.5:0.9, add dibutyltin dilaurate, stir for 2.5 hours at a temperature of 55° C. and a stirring speed of 180 r / min, then cool to 35° C., add the polyvinyl alcohol solution prepared in step S2, wherein the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 8:1.5, react for 25 minutes, and obtain modified polyvinyl alcohol B;

[0106] Step S4. 25 g of octamethylcyclotetrasiloxane, 1.75 g of KH-551, 9 g of methyldimethoxydodecylsilane, 0.045 g of tetramethylammonium hydroxide and 26 g of 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane were reacted in an oil bath at 90° C. for 5.5 h, and then the system temperature was raised to 135° C. and kept at reflux for 40 min. Low boiling substances were removed under reduced pressure to obtain amino silicone oil;

[0107] Step S5. Mixing amino silicone oil and maleic anhydride in a molar ratio of 1:1 between the amino group in the amino silicone oil and the maleic anhydride, heating to 65° C., and reacting for 40 min to obtain an auxiliary agent;

[0108] Step S6. 35 g of the base polyvinyl alcohol solution, 4.9 g of modified polyvinyl alcohol A, 4.9 g of modified polyvinyl alcohol B and 3 g of the additive were mixed evenly, and heated at 85° C. for 1 h to obtain glue solution B;

[0109] Step S7. After fixing the paper, use a coating machine to apply sizing liquid B on the surface at a sizing rate of 3.0 mm / s, and then dry at 50° C. for 13 minutes to obtain sizing liquid B sizing paper;

[0110] Step S8. dissolving the organic boric acid modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.01 wt%, immersing the sizing paper of sizing solution B in the aqueous solution for 8 min, washing it with a 2 mM NaCl deionized water solution, and drying it at 25° C. for 5 min to obtain a sizing agent coated on the surface of the paper.

[0111] Performance Test:

[0112] Paper folding test:

[0113] According to GB / T457-2008 standard, the folding resistance of paper was tested. The paper coated with sizing agent on the surface prepared in Example 1 to Example 6 and Comparative Example 1 to Comparative Example 5 was tested longitudinally and transversely. The size of the paper sample was 15 mm × 100 mm. The double folding times were tested three times respectively, and the average value was taken.

[0114] Paper tensile index test:

[0115] The tensile strength is the resistance of paper when it is subjected to tension only. The force required for its breakage is called the tensile strength. The tensile strength of paper is tested with reference to GB / T12914-2008 standard. The tensile strength of the paper coated with sizing agent on the surface prepared in Examples 1 to 6 and Comparative Examples 1 to 5 is tested using a ZL-100A / 300A paper and paperboard tensile testing machine. The sample size is 250 mm × 15 mm. The test is repeated three times and the average value is taken. The tensile index is calculated as follows:

[0116] ;

[0117] Where Y is the tensile index, in N·m·g -1 ; F is the average tensile strength, in N; Lw is the width of the paper, in mm; g is the basis weight of the paper, in g / m 2 ;

[0118] Paper tearing index test:

[0119] The tear strength of the paper coated with sizing agent on the surface of the paper cups in Examples 1 to 6 and Comparative Examples 1 to 5 was tested according to GB / T455-2002 standard. The sample size was 63 mm × 75 mm. The average value was taken after three tests. The tear index calculation formula is:

[0120] ;

[0121] Where X is the tear index, in mN·m 2 ·g -1; T is the tear strength, unit is mN; g is the weight of the sample paper, unit is 80g / m 2 ;

[0122] Paper bursting index test:

[0123] Referring to GB / T454-2002 standard, the bursting resistance of the paper coated with the sizing agent on the surface prepared in Examples 1 to 6 and Comparative Examples 1 to 5 was tested. The bursting resistance was tested using an NPD-D paper bursting resistance tester. The size of the paper sample was 70 mm × 70 mm. After multiple measurements, the average value was taken, and the bursting resistance index was calculated according to the formula:

[0124] ;

[0125] Where x is the burst resistance index, in kPa·m 2 ·g -1 ; P is bursting strength, unit is kPa; g is the basis weight of the sample paper, unit is 80g / m 2 ;

[0126] Water resistance test of paper:

[0127] Contact angle measurement:

[0128] At room temperature, the paper with the sizing agent coated on the surface prepared in Examples 1 to 6 and Comparative Examples 1 to 5 was cut into pieces of 10 mm×15 mm, and a DSA100 optical contact angle measuring instrument produced by KRUSS was used to perform a dynamic contact angle test on the samples using a hanging drop method;

[0129] Wet tensile strength test of paper:

[0130] The paper coated with sizing agent on the surface prepared in Examples 1 to 6 and Comparative Examples 1 to 5 was made into samples with a size of 15 mm × 100 mm, each group of samples was put into water and soaked for 10 minutes, then taken out, the surface moisture of the sizing paper was absorbed with filter paper, and the wet tensile strength test was performed;

[0131] Ink adhesion test of paper:

[0132] According to the ASTM standard, the ink adhesion test was carried out on the sized paper with the sizing agent coated on the surface prepared in Examples 1 to 6 and Comparative Examples 1 to 5, wherein the ink shedding area ratio (A) after the test was qualified at the ink adhesion level 4B or 5B; when A=0, there was no ink shedding, which was recorded as level 5B; when 0<A<5%, it was recorded as level 4B; when 5%<A<15%, it was recorded as level 3B; when 15%<A<35%, it was recorded as level 2B; when 35%<A<65%, it was recorded as level 1B; when 65%<A<100%, it was recorded as level 0B. The results are shown in Tables 1 and 2 below:

[0133] Table 1 Summary of some raw materials and amounts in Examples 1 to 6 and Comparative Examples 1 to 5

[0134] ;

[0135] Table 2 Summary of performance test results in Examples 1 to 6 and Comparative Examples 1 to 5

[0136] ;

[0137] Data Analysis:

[0138] It can be seen from Table 1 and Table 2 that the paper with the sizing agent coated on the surface prepared by the present invention has higher folding endurance, greater tensile strength, greater bursting resistance index, greater tear index and ink adhesion. This may be because the sizing solution A provided in the present invention is first used to soak the paper and then the sizing solution B is coated on the surface. The boric acid structure in the sizing solution A can be cross-linked with the active groups such as hydroxyl groups in the paper fiber and the sizing solution B at the same time, thereby forming a multiple network structure. The formation of the network structure can increase the density of the paper, prevent the ink from excessively diffusing during the writing process, and improve the water-blocking effect of the paper, which improves the strength of the paper. In addition, the network structure synergizes with the carboxyl group in the boric acid structure, so that the ink can be dispersed in the gaps of the network structure inside the system, which helps to improve the adhesion of the paper to the ink. On the contrary, when the sizing solution A and the sizing solution B are switched in order, the various properties of the paper are reduced.

[0139] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0140] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A safe and environmentally friendly sizing agent for papermaking, characterized in that: The sizing agent comprises a glue layer A and a glue layer B which are sequentially coated on the surface of the paper; The glue layer A is obtained by coating glue liquid A on the surface of paper, and the glue layer B is obtained by coating glue liquid B on the surface of the glue layer A, and the mass ratio of the glue liquid A to the glue liquid B is 0.2-0.25:2.5-3; The glue A is prepared by modifying polyvinyl amine with organic boric acid; The glue solution B comprises the following raw materials in parts by weight: 35-45 parts of base polyvinyl alcohol solution, 4.9-5.15 parts of modified polyvinyl alcohol A, 4.9-5.15 parts of modified polyvinyl alcohol B, and 3-3.25 parts of additives; The concentration of the matrix polyvinyl alcohol solution is 8%-10%; The modified polyvinyl alcohol A is polyvinyl alcohol modified by a silane coupling agent; The modified polyvinyl alcohol B is isocyanate-modified polyvinyl alcohol; The auxiliary agent is carboxyl silane; The preparation method of the modified polyvinyl alcohol A is as follows: Add polyvinyl alcohol to deionized water, stir at 85-90°C for 1.5-2h to obtain a polyvinyl alcohol solution, then cool to 55-60°C, dropwise add KH-560, and adjust the pH value of the reaction system to 7-8 with 10% sodium hydroxide solution, and then stir at 190-200r / min for 1.5-2h to obtain modified polyvinyl alcohol A; The concentration of the polyvinyl alcohol solution is 8%-10%, and the mass ratio of the polyvinyl alcohol solution to KH-560 is 8-9:1.25-1.5; The preparation method of the modified polyvinyl alcohol B is as follows: Step A1. Add polyvinyl alcohol to toluene and stir at 85-90° C. for 3.5-4 h to obtain a polyvinyl alcohol solution; Step A2. Mix butanone oxime and isophorone diisocyanate, add dibutyltin dilaurate, stir at a temperature of 55-60°C and a stirring speed of 180-200 r / min for 2.5-3h, then cool to 35-40°C, add the polyvinyl alcohol solution prepared in step A1, and react for 25-30min to obtain modified polyvinyl alcohol B; The concentration of the polyvinyl alcohol solution in step A1 is 16%-18%; The molar ratio of butanone oxime to isophorone diisocyanate in step A2 is 1.5-2:0.9-1.15, and the mass ratio of polyvinyl alcohol to isophorone diisocyanate is 8-10:1.5-2; The preparation method of the carboxyl silane is as follows: Step B1. react octamethylcyclotetrasiloxane, KH-551, methyldimethoxydodecylsilane, tetramethylammonium hydroxide and 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane in an oil bath at 90-100°C for 5.5-6h, then raise the system temperature to 135-140°C, maintain reflux for 40-60min, remove low boiling points under reduced pressure, and obtain amino silicone oil; Step B2. Mix the amino silicone oil and maleic anhydride, heat to 65-70°C, and react for 40-60 minutes to obtain carboxyl silane; The mass ratio of octamethylcyclotetrasiloxane, KH-551, methyldimethoxydodecylsilane, tetramethylammonium hydroxide and 1,3,5-tris(methyltrifluoropropyl)cyclotrisiloxane in step B1 is 25-30:1.75-2:9-11:0.045-0.05:26-28; The molar ratio of amino group to maleic anhydride in the amino silicone oil in step B2 is 1:1-1.

05.

2. The safe and environmentally friendly papermaking sizing agent according to claim 1, characterized in that: The preparation method of the sizing agent is as follows: Step S1. dissolving the organic boric acid modified polyethylene amine in deionized water to prepare an aqueous solution with a concentration of 0.01wt%-0.015wt%, immersing the paper in the aqueous solution for 8-10 minutes, then washing the paper with a 2mM NaCl deionized water solution, and then drying the paper at 25-30°C for 5-7 minutes to obtain sizing solution A sizing paper; Step S2. The base polyvinyl alcohol solution, modified polyvinyl alcohol A, modified polyvinyl alcohol B and the additive are mixed evenly, and heated at 85-90° C. for 1-2 h to obtain glue solution B; Step S3. Fix the sizing liquid A coated paper and use a coating machine to apply sizing liquid B at a sizing rate of 3.0-4.0 mm / s to apply sizing to the surface. Put the sizing paper into a constant temperature box and dry it at a temperature of 50-60° C. for 13-15 minutes to obtain the sizing agent coated on the surface of the paper.

Citation Information

Patent Citations

  • Rice starch sizing agent

    CN108824079A

  • A method for preparing alkyl ketene dimers

    CN114539190B

  • Super-hydrophobic paper and paper making method thereof

    CN106400585A

  • Hydrophobic surface wetting method and wetting agent

    CN110028893A