A preparation method of composite solid electrolyte membrane and its application
By designing a composite solid electrolyte membrane with a composite structure, the problem of insufficient mechanical properties and ion conduction capabilities of the electrolyte membrane in all-solid-state lithium batteries is solved, a high-performance electrolyte membrane is achieved, and the cycle life and capacity retention rate of the battery are significantly improved. .
Patent Information
- Application Number
- CN202411017712.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing all-solid-state lithium battery composite solid electrolyte membranes have problems such as poor interfacial stability, low ionic conductivity, insufficient mechanical properties, complex manufacturing processes, poor thermal stability, and poor electrochemical stability, which limit their practical applications. performance and lifespan.
Design a composite solid electrolyte membrane with a composite structure. Nanoscale fillers and modified polymer molecular structures are used to improve ionic conductivity and mechanical strength, and additives are added to the electrolyte to adjust interfacial compatibility to form a high-performance composite Solid electrolyte membrane.
The good mechanical properties and ion transmission performance of the composite solid electrolyte membrane are achieved, and the capacity is maintained at more than 90% after 50 cycles, significantly improving the cycle life.
Smart Images

Figure CN118538989B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of all-solid-state soft-pack battery electrolyte membrane materials. Specifically, the present invention relates to a preparation method of a composite solid electrolyte membrane and its application, specifically to an all-solid-state soft-pack battery, and also to a preparation method of an all-solid-state soft-pack battery containing the composite electrolyte membrane. Background Art
[0002] As the research on all-solid-state lithium batteries continues to deepen, the research on composite solid electrolyte membranes has also made significant progress. However, there are still problems such as poor interface stability, low ionic conductivity, insufficient mechanical properties, complex manufacturing process, poor thermal stability, large interface resistance and poor electrochemical stability, which limit its performance and life in practical applications.
[0003] In view of the above problems, a composite solid electrolyte membrane with a composite structure is designed to improve the mechanical properties and flexibility of the membrane. The ion conductivity of the solid electrolyte is improved by using nano-scale fillers, controlling the pore size and specific surface area of the fillers, etc. For the composite polymers present in the solid electrolyte, the ion affinity and ion conductivity of the polymer are improved by modifying the molecular structure of the polymer and introducing polar groups, and the mechanical strength of the composite solid electrolyte membrane is improved. Adding additives to the composite electrolyte can adjust the interface compatibility between the filler and the polymer matrix and increase the probability of forming ion transmission channels. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a composite solid electrolyte membrane and its application in view of the problems existing in the prior art. The composite solid electrolyte membrane of the present invention has the following advantages: good mechanical properties (tensile strength 12MPa) and ion transport properties (11.2 mS / cm), and can maintain more than 90% of the capacity after 50 cycles in all-solid-state soft-pack batteries, and the cycle life is greatly improved.
[0005] To achieve the above purpose, the present invention adopts the following technical solution:
[0006] The present invention provides a method for preparing a composite solid electrolyte membrane, comprising the following steps:
[0007] S1. Preparation of composite polymer electrolyte slurry:
[0008] Adding the polymer to the solvent, adding the lithium salt, and stirring to obtain a uniform composite polymer electrolyte slurry;
[0009] S2. Preparation of composite solid electrolyte membrane:
[0010] The solvent-modified electrolyte mixture is added into the composite polymer electrolyte slurry, and an inorganic additive is added and mixed evenly to obtain a mixed slurry; the mixed slurry is coated on a carrier, and the composite solid electrolyte membrane is obtained after drying.
[0011] As an embodiment of the present invention, in the mixed slurry in step S2, the mass proportions of the components are: 50-80% of the co-solvent-modified sulfide electrolyte, 15-40% of the composite polymer electrolyte, and 5-10% of the inorganic additive.
[0012] The co-solvent modified sulfide electrolyte is a co-solvent coated sulfide electrolyte;
[0013] The composite polymer electrolyte comprises lithium salt and polymer.
[0014] As an embodiment of the present invention, in step S2, the co-solvent-modified sulfide electrolyte is prepared by the following method: adding sulfide electrolyte powder to the co-solvent, evenly dispersing it, sealing it and letting it stand for 10-24 hours, so that the co-solvent forms a coating layer on the surface of the sulfide electrolyte powder, and filtering out excess co-solvent to obtain the co-solvent-modified sulfide electrolyte.
[0015] Preferably, the sulfide electrolyte is one or more of crystalline sulfide electrolytes; the crystalline sulfide electrolyte includes one of Thio-LISICON type, LGPS type, and Argentum type.
[0016] Preferably, the particle size of the sulfide electrolyte is 50-400 μm. In order to obtain a uniform mixture and increase the reaction area, the sulfide electrolyte powder needs to be crushed and ground, and a ball mill, a grinder or the like can be used for crushing, and the crushed powder is sieved and graded to obtain a uniform powder with a particle size in the range of 50-400 μm.
[0017] Preferably, the co-solvent includes one or more of N-methylpyrrolidone (NMP) and dimethyl sulfoxide (DMSO).
[0018] Preferably, the mass ratio of the co-solvent to the sulfide electrolyte powder is 2-3:7-8.
[0019] Preferably, the uniform dispersion method is ultrasonic dispersion or mechanical stirring. The uniform dispersion time is 6-10 hours. The cosolvent forms a 5-10 nm uniform and stable coating layer on the powder surface. The frequency of ultrasonic dispersion is controlled between 30-100 kHz, and the speed of mechanical stirring is controlled between 400-800 rpm. Long-term dispersion can make the solvent fully coated on the powder surface, which is convenient for the formation of the coating layer later.
[0020] Preferably, the standing time is 15-24 hours. The filtration is to filter out the excess co-solvent to obtain the electrolyte powder with the coating layer formed only on the surface of the sulfide electrolyte powder.
[0021] The key to the formation of the coating layer is to disperse it first (ultrasonic dispersion or mechanical stirring) and then stand it for a long time. The difficulty is to form a uniform coating layer. Dispersing it first can make the sulfide electrolyte powder particles evenly dispersed in the co-solvent. Sufficient standing time (10-24 h) can allow the co-solvent to slowly infiltrate the surface of the powder particles and gradually form a coating layer. However, filtering immediately after mixing will not form a uniform coating layer, and there may even be only an incomplete half-coating layer, and the layer structure is also unstable. In the subsequent preparation, the coating layer will quickly dissolve in the solvent, and the solubility of the sulfide electrolyte powder in the composite polymer electrolyte slurry cannot be improved.
[0022] As an embodiment of the present invention, in step S1, the polymer includes a combination of two or more of polyethylene oxide (PEO), polycarbonate (PC), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), poly(ethylene-propylene-butadiene) rubber (EPDM), sulfonated polyphenylene ether (SPES), poly(ethylene-ethylene oxide) copolymer (PEO-POX), poly(ethyleneimine) (PEI), poly(ionic liquid) (PIL), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP). The present invention uses two or more polymers, and different polymers can form a macromolecular cross-linked polymer network to stabilize the lithium ion conduction channel.
[0023] As an embodiment of the present invention, in step S1, the lithium salt includes one or a combination of lithium hexafluorophosphate (LiPF6), lithium chlorofluorosulfonate (LiFSO3CF3), lithium trifluoromethanesulfonate (LiCF3SO3), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium fluorosulfonate (LiFSO3), lithium ethylene sulfonate (LiES), lithium trifluoroacetate (LiTFA), lithium tetrafluoroacetate (LiFBA), lithium pentafluoroacetate (LiPFBA), and lithium bis(fluorosulfonyl)imide (LiTFSI).
[0024] As an embodiment of the present invention, in step S1, in the composite polymer electrolyte, the mass ratio of polymer to lithium salt is 2-3: 1. The composite polymer electrolyte includes at least two polymers, wherein the mass proportion of each polymer in the total amount of polymers is at least 10%.
[0025] As an embodiment of the present invention, in step S2, the inorganic additive is selected from one of SiO2 and Al2O3.
[0026] As an embodiment of the present invention, in step S1, the mass ratio of the polymer, the solvent and the lithium salt is 2:1:1-3:3:1.
[0027] As one embodiment of the present invention, the solvent includes one or more of ethylene glycol methyl ether (DGM), propylene glycol methyl ether (PGME), 1,3-dioxolane (THF), triethyl phosphate (TEP), tetramethyl urea (TMU), ethyl trifluoromethanesulfonate (EMTF), butyl tetrafluoroacetate (DBE), and propyl pentafluoroacetate (PFP).
[0028] As an embodiment of the present invention, in step S1, the stirring time is 6-10 hours.
[0029] As an embodiment of the present invention, in step S2, the mixing can be carried out using a mixer, a grinder, a shearing machine and the like for 10-15 hours, and the uniformity of the mixture is ensured.
[0030] As an embodiment of the present invention, in step S2, the carrier is a copper strip or an aluminum strip. The coating is to place the mixed slurry in a glove box and use a coating machine to evenly coat the slurry with a scraper.
[0031] As an embodiment of the present invention, in step S2, the drying time is 6-20 hours. After drying, the composite solid electrolyte membrane is formed on the copper strip or the aluminum strip.
[0032] The present invention also provides an application of a composite solid electrolyte membrane in an all-solid-state soft-pack battery.
[0033] The present invention also provides an all-solid-state soft-pack battery, comprising a lithium metal negative electrode or a metal lithium composite negative electrode, a positive electrode and the composite solid electrolyte membrane.
[0034] Compared with the composite solid electrolyte membrane in the prior art, the beneficial effects of the present invention are:
[0035] (1) The addition of a co-solvent forms a coating layer on the surface of the sulfide electrolyte particles, which can improve the solubility of the electrolyte in the solvent. That is, the composite polymer electrolyte slurry can better dissolve the sulfide solid electrolyte, which helps to evenly mix and disperse the electrolyte materials, and provides a basis for enhancing ionic conductivity, improving interface stability, and improving the processing performance of the electrolyte materials.
[0036] (2) Modification of polymer matrix: the added lithium salt improves the ion affinity and ion conductivity of the polymer. Additives adjust the interfacial compatibility between the sulfide electrolyte with the coating layer and the polymer matrix, increasing the probability of forming ion transport channels. Composite electrolyte membrane structure: A composite solid electrolyte membrane with a composite structure (a macromolecular cross-linked polymer network formed by multiple polymers) can improve the mechanical properties and flexibility of the membrane.
[0037] (3) Composite solid electrolyte membrane used in the present invention The composite solid electrolyte membrane of the present invention has both good mechanical properties and ion transport properties, and realizes high-performance all-solid-state soft-pack batteries. The preparation method is simple and easy, the cost is low, and it is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0039] Figure 1 The capacity retention rate curve of the all-solid-state soft-pack lithium metal battery assembled from the products prepared in Example 1 and Comparative Example 1 is shown. DETAILED DESCRIPTION
[0040] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0041] Example 1
[0042] This embodiment provides a preparation method of a composite solid electrolyte membrane, and the preparation steps are as follows:
[0043] The sulfide electrolyte is Li6PS5Cl; the co-solvent is N-methylpyrrolidone (NMP); the polymer is polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and polyvinylidene fluoride (PVDF), the Li salt is bis(fluorosulfonyl imide) lithium (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is Al2O3;
[0044] Its preparation method is:
[0045] S1. Add the predetermined PVDF-HFP and PVDF into the solvent DGM, and the weight ratio of PVDF-HFP, PVDF and DGM is 1:1:1.
[0046] S2. Add LiTFSI (weight ratio [(PVDF-HFP)+PVDF] / LiTFSI is 2:1) and continue stirring for 6 hours to prepare a uniform slurry.
[0047] S3. In order to obtain a uniform mixture and increase the reaction area, the Li6PS5Cl sulfide electrolyte powder needs to be crushed and ground. The powder is crushed using a ball mill or other equipment, and the crushed powder is sieved and graded to obtain a powder with a particle size of 50-400 μm.
[0048] S4, Li6PS5Cl powder was dispersed in NMP, and then mechanically stirred at 500 rpm for 6 h to allow NMP to fully form a uniform NMP coating layer on the powder surface, and filtered after standing for 15 h. The mass ratio of NMP cosolvent to sulfide electrolyte before mixing was 3:7.
[0049] S5, add the NMP-modified Li6PS5Cl mixture to the slurry in S2 and control the mass ratio of the mixture to the composite polymer electrolyte to be 4:1 (76%:19%), and add 5% Al2O3 for uniform mixing. Use a mixer to mix for 10 hours to ensure the uniformity of the mixture.
[0050] S6. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on the copper tape using a scraper, and let it stand for 6 hours, so that a composite solid electrolyte membrane is formed on the copper tape.
[0051] Example 2
[0052] This embodiment provides a preparation method of a composite solid electrolyte membrane, and the preparation steps are as follows:
[0053] The sulfide electrolyte is Li 10 GeP2S 12 ; The cosolvent is N-methylpyrrolidone (NMP); the polymer is polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and polyvinylidene fluoride (PVDF), the Li salt is bis(fluorosulfonyl imide) lithium (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is Al2O3;
[0054] Its preparation method is:
[0055] S1. Add the predetermined PVDF-HFP and PVDF into the solvent DGM, and the weight ratio of PVDF-HFP, PVDF and DGM is 1:1:1.
[0056] S2. Add LiTFSI (weight ratio [(PVDF-HFP)+PVDF] / LiTFSI is 2:1) and continue stirring for 6 hours to prepare a uniform slurry.
[0057] S3. In order to obtain a uniform mixture and increase the reaction area, Li 10 GeP2S 12 The sulfide electrolyte powder is crushed and ground. A ball mill, a grinder or the like can be used for the crushing, and the crushed powder is sieved and classified to obtain a powder with uniform particle size.
[0058] S4. Li 10 GeP2S 12 The powder was dispersed in NMP and then mechanically stirred at 500 rpm for 6 h to allow NMP to fully form a uniform NMP coating layer on the powder surface, and filtered after standing for 15 h. The mass ratio of NMP cosolvent to sulfide electrolyte before mixing was 3:7.
[0059] S5, Li modified by NMP 10 GeP2S 12 The mixture was added to the slurry in S2 and the mass ratio with the composite polymer electrolyte was controlled to be 4:1, and 5% Al2O3 was added for uniform mixing. The mixture was mixed for 10 hours using a mixer to ensure the uniformity of the mixture.
[0060] S6. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on the copper tape using a scraper, and let it stand for 6 hours, so that a composite solid electrolyte membrane is formed on the copper tape.
[0061] Example 3
[0062] This embodiment provides a preparation method of a composite solid electrolyte membrane and its application in an all-solid-state soft-pack battery. The preparation steps are as follows:
[0063] Sulfide electrolyte is Li7P3S 11 ; The cosolvent is N-methylpyrrolidone (NMP); the polymer is polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and polyvinylidene fluoride (PVDF), the Li salt is bis(fluorosulfonyl imide) lithium (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is Al2O3;
[0064] Its preparation method is:
[0065] S1. Add the predetermined PVDF-HFP and PVDF into the solvent DGM, and the weight ratio of PVDF-HFP, PVDF and DGM is 1:1:1.
[0066] S2. Add LiTFSI (weight ratio [(PVDF-HFP)+PVDF] / LiTFSI is 2:1) and continue stirring for 6 hours to prepare a uniform slurry.
[0067] S3. In order to obtain a uniform mixture and increase the reaction area, Li7P3S 11 The sulfide electrolyte powder is crushed and ground. A ball mill, a grinder or the like can be used for the crushing, and the crushed powder is sieved and classified to obtain a powder with uniform particle size.
[0068] S4, Li7P3S 11 The powder was dispersed in NMP and then mechanically stirred at 500 rpm for 6 h to allow NMP to fully form a uniform NMP coating layer on the powder surface, and filtered after standing for 15 h. The mass ratio of NMP cosolvent to sulfide electrolyte before mixing was 3:7.
[0069] S5, Li7P3S modified by NMP 11 The mixture was added to the slurry in S2 and the mass ratio with the composite polymer electrolyte was controlled to be 4:1, and 5% Al2O3 was added. The mixture was mixed for 10 hours using a mixer to ensure the uniformity of the mixture.
[0070] S6. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on the copper tape using a scraper, and let it stand for 6 hours, so that a composite solid electrolyte membrane is formed on the copper tape.
[0071] Example 4
[0072] This embodiment provides a preparation method of a composite solid electrolyte membrane, and the preparation steps are as follows:
[0073] The sulfide electrolyte is Li6PS5Cl; the cosolvent is dimethyl sulfoxide (DMSO); the polymer is polyethylene oxide (PEO) and polyacrylonitrile (PAN), the Li salt is lithium bis(fluorosulfonyl imide) (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is SiO2;
[0074] Its preparation method is:
[0075] S1. Add the predetermined PEO and PAN into the solvent DGM, and the weight ratio of PEO, PAN and DGM is 1:1:2.
[0076] S2. Add LiTFSI (weight ratio [PEO+PAN] / LiTFSI is 3:1) and stir continuously for 6 hours to prepare a uniform slurry.
[0077] S3. In order to obtain a uniform mixture and increase the reaction area, the Li6PS5Cl sulfide electrolyte powder needs to be crushed and ground. The powder is crushed using a ball mill or other equipment, and the crushed powder is sieved and graded to obtain a powder with a particle size of 50-400 μm.
[0078] S4, Li6PS5Cl powder was dispersed in DMSO, and then mechanically stirred at 500 rpm for 6 h to allow DMSO to fully form a uniform DMSO coating layer on the powder surface, and filtered after standing for 20 h. The mass ratio of DMSO cosolvent to sulfide electrolyte before mixing was 2:8.
[0079] S5, add the NMP-modified Li6PS5Cl mixture to the slurry in S2 and control the mass ratio of the mixture to the composite polymer electrolyte to be 2:1 (60%:30%), and add 10% Al2O3 for uniform mixing. Use a mixer to mix for 10 hours to ensure the uniformity of the mixture.
[0080] S6. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on the copper tape using a scraper, and let it stand for 6 hours, so that a composite solid electrolyte membrane is formed on the copper tape.
[0081] Example 5
[0082] This embodiment provides a preparation method of a composite solid electrolyte membrane, and the preparation steps are as follows:
[0083] The sulfide electrolyte is Li6PS5Cl; the cosolvent is dimethyl sulfoxide (DMSO); the polymer is polyethylene oxide (PEO) and polyacrylonitrile (PAN), the Li salt is lithium bis(fluorosulfonyl imide) (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is SiO2;
[0084] Its preparation method is:
[0085] S1. Add the predetermined PEO and PAN into the solvent DGM, and the weight ratio of PEO, PAN and DGM is 0.2:1.8:2.
[0086] S2. Add LiTFSI (weight ratio [PEO + PAN] / LiTFSI is 3:1) and continue stirring for 6 hours to prepare a uniform slurry.
[0087] S3. In order to obtain a uniform mixture and increase the reaction area, the Li6PS5Cl sulfide electrolyte powder needs to be crushed and ground. The powder is crushed using a ball mill or other equipment, and the crushed powder is sieved and graded to obtain a powder with a particle size of 50-400 μm.
[0088] S4, Li6PS5Cl powder was dispersed in DMSO, and then mechanically stirred at 500 rpm for 6 h to allow DMSO to fully form a uniform DMSO coating layer on the powder surface, and filtered after standing for 10 h. The mass ratio of DMSO cosolvent to sulfide electrolyte before mixing was 2:8.
[0089] S5, add the NMP-modified Li6PS5Cl mixture to the slurry in S2 and control the mass ratio of the NMP-modified Li6PS5Cl mixture to the composite polymer electrolyte to be 5:4 (50%:40%), and add 10% Al2O3 for uniform mixing. Use a mixer to mix for 10 hours to ensure the uniformity of the mixture.
[0090] S6. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on the copper tape using a scraper, and let it stand for 6 hours, so that a composite solid electrolyte membrane is formed on the copper tape.
[0091] Example 6
[0092] This embodiment provides a preparation method of a composite solid electrolyte membrane, and the preparation steps are as follows:
[0093] The sulfide electrolyte is Li6PS5Cl; the cosolvent is dimethyl sulfoxide (DMSO); the polymer is polyethylene oxide (PEO) and polyacrylonitrile (PAN), the Li salt is lithium bis(fluorosulfonyl imide) (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is SiO2;
[0094] Its preparation method is:
[0095] S1. Add the predetermined PEO and PAN into the solvent DGM, and the weight ratio of PEO, PAN and DGM is 1.8:0.2:2.
[0096] S2. Add LiTFSI (weight ratio [PEO+PAN] / LiTFSI is 3:1) and stir continuously for 6 hours to prepare a uniform slurry.
[0097] S3. In order to obtain a uniform mixture and increase the reaction area, the Li6PS5Cl sulfide electrolyte powder needs to be crushed and ground. The powder is crushed using a ball mill or other equipment, and the crushed powder is sieved and graded to obtain a powder with a particle size of 50-400 μm.
[0098] S4, disperse Li6PS5Cl powder in DMSO, and then stir mechanically at 500rpm for 6 hours to allow DMSO to fully form a uniform DMSO coating layer on the powder surface, and filter after standing for 24 hours. The mass ratio of DMSO cosolvent to sulfide electrolyte before mixing is 2:8.
[0099] S5, add the NMP-modified Li6PS5Cl mixture to the slurry in S2 and control the mass ratio of the mixture to the composite polymer electrolyte to be 16:3 (80%:15%), and add 5% Al2O3 for uniform mixing. Use a mixer to mix for 24 hours to ensure the uniformity of the mixture.
[0100] S6. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on the copper tape using a scraper, and let it stand for 6 hours, so that a composite solid electrolyte membrane is formed on the copper tape.
[0101] Comparative Example 1
[0102] This comparative example provides a preparation of a sulfide-free electrolyte composite solid electrolyte membrane and its application in an all-solid-state soft-pack battery. The preparation steps are as follows:
[0103] The polymer is polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and polyvinylidene fluoride (PVDF), the Li salt is lithium bis(fluorosulfonyl imide) (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is Al2O3;
[0104] Its preparation method is:
[0105] S1. Add the predetermined PVDF-HFP and PVDF into the solvent DGM, and the weight ratio of PVDF-HFP, PVDF and DGM is 1:1:1.
[0106] S2. Add LiTFSI (weight ratio [(PVDF-HFP)+PVDF] / LiTFSI is 2:1) and add 5% Al2O3, and stir continuously for 6 hours to make a uniform slurry.
[0107] S3. Place the slurry in a glove box, use a coating machine to evenly coat the slurry on a copper strip using a scraper, and let it stand for 6 hours, so that a polymer solid electrolyte membrane is formed on the copper strip.
[0108] Comparative Example 2
[0109] This comparative example provides a preparation of a sulfide-free electrolyte composite solid electrolyte membrane and its application in an all-solid-state soft-pack battery. The preparation steps are as follows:
[0110] The polymer is PVDF, the Li salt is lithium bis(fluorosulfonyl imide) (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is Al2O3;
[0111] Its preparation method is:
[0112] S1. Add the predetermined PVDF into the solvent DGM, and the weight ratio of PVDF to DGM is 1:1.
[0113] S2. Add LiTFSI (weight ratio of PVDF / LiTFSI is 2:1) and add 5% Al2O3, and stir continuously for 6 hours to prepare a uniform slurry.
[0114] S3. Place the slurry in a glove box, use a coating machine to evenly coat the slurry on a copper tape using a scraper, and let it stand for 6 hours, so that a polymer electrolyte membrane is formed on the copper tape.
[0115] Comparative Example 3
[0116] This comparative example provides a preparation of a sulfide-free electrolyte composite solid electrolyte membrane and its application in an all-solid-state soft-pack battery. The preparation steps are basically the same as those in Example 1, except that the polymer is only PVDF and the total amount remains unchanged.
[0117] The sulfide electrolyte is Li6PS5Cl; the co-solvent is N-methylpyrrolidone (NMP); the polymer is polyvinylidene fluoride (PVDF), the Li salt is bis(fluorosulfonyl imide) lithium (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is Al2O3;
[0118] Its preparation method is:
[0119] S1. Add the predetermined PVDF into the solvent DGM, and the weight ratio of PVDF to DGM is 1:1.
[0120] S2. Add LiTFSI (weight ratio of PVDF / LiTFSI is 2:1) and stir continuously for 6 hours to prepare a uniform slurry.
[0121] S3. In order to obtain a uniform mixture and increase the reaction area, the Li6PS5Cl sulfide electrolyte powder needs to be crushed and ground. The powder is crushed using a ball mill or other equipment, and the crushed powder is sieved and graded to obtain a powder with a particle size of 50-400 μm.
[0122] S4, Li6PS5Cl powder was dispersed in NMP, and then mechanically stirred at 500 rpm for 6 h to allow NMP to fully form a uniform NMP coating layer on the powder surface, and filtered after standing for 15 h. The mass ratio of NMP cosolvent to sulfide electrolyte before mixing was 3:7.
[0123] S5, adding the NMP-modified Li6PS5Cl mixture to the slurry in S2 and controlling the mass ratio to be 4:1, adding 5% Al2O3, and mixing for 10 hours using a mixer to ensure the uniformity of the mixture.
[0124] S6. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on the copper tape using a scraper, and let it stand for 6 hours, so that a composite solid electrolyte membrane is formed on the copper tape.
[0125] Comparative Example 4
[0126] This comparative example provides a preparation method of a sulfide-free electrolyte composite solid electrolyte membrane and its application in an all-solid-state soft-pack battery. The preparation steps are basically the same as those in Example 1, except that the Li6PS5Cl powder and the co-solvent NMP are not mixed in advance but directly added to the slurry.
[0127] The sulfide electrolyte is Li6PS5Cl; the co-solvent is N-methylpyrrolidone (NMP); the polymer is polyvinylidene fluoride-hexafluoropropylene P (VDF-HFP) and polyvinylidene fluoride (PVDF), the Li salt is bis(fluorosulfonyl imide) lithium (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is Al2O3;
[0128] Its preparation method is:
[0129] S1. Add the predetermined PVDF-HFP and PVDF into the solvent DGM, and the weight ratio of PVDF-HFP, PVDF and DGM is 1:1:1.
[0130] S2. Add LiTFSI (weight ratio [P(VDF-HFP)+PVDF] / LiTFSI is 2:1) and stir continuously for 6 hours to prepare a uniform slurry.
[0131] S3. In order to obtain a uniform mixture and increase the reaction area, the Li6PS5Cl sulfide electrolyte powder needs to be crushed and ground. The powder is crushed using a ball mill or other equipment, and the crushed powder is sieved and graded to obtain a powder with a particle size of 50-400 μm.
[0132] S4, add NMP cosolvent and Li6PS5Cl electrolyte (mass ratio of 3:7) to the slurry in S2 and control the mass ratio to 4:1, add 5% Al2O3. Use a mixer to mix for 10 hours to ensure the uniformity of the mixture.
[0133] S5. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on a copper strip with a scraper, and dry for 6 hours to form a composite solid electrolyte membrane on the copper strip.
[0134] Comparative Example 5
[0135] This comparative example provides a preparation method of a sulfide-free electrolyte composite solid electrolyte membrane and its application in an all-solid-state soft-pack battery. The preparation steps are basically the same as those in Example 1, except that Li6PS5Cl powder is dispersed in NMP and directly added to the slurry without standing after stirring.
[0136] The sulfide electrolyte is Li6PS5Cl; the co-solvent is N-methylpyrrolidone (NMP); the polymer is polyvinylidene fluoride-hexafluoropropylene P (VDF-HFP) and polyvinylidene fluoride (PVDF), the Li salt is bis(fluorosulfonyl imide) lithium (LiTFSI); the solvent is ethylene glycol methyl ether (DGM), and the inorganic additive is Al2O3;
[0137] Its preparation method is:
[0138] S1. Add the predetermined PVDF-HFP and PVDF into the solvent DGM, and the weight ratio of PVDF-HFP, PVDF and DGM is 1:1:1.
[0139] S2. Add LiTFSI (weight ratio [P(VDF-HFP)+PVDF] / LiTFSI is 2:1) and stir continuously for 6 hours to prepare a uniform slurry.
[0140] S3. In order to obtain a uniform mixture and increase the reaction area, the Li6PS5Cl sulfide electrolyte powder needs to be crushed and ground. The powder is crushed using a ball mill or other equipment, and the crushed powder is sieved and graded to obtain a powder with a particle size of 50-400 μm.
[0141] S4, Li6PS5Cl powder was dispersed in NMP, and then mechanically stirred at 500 rpm for 6 h, and then filtered. The mass ratio of NMP co-solvent to sulfide electrolyte before mixing was 3:7.
[0142] S5, Li7P3S modified by NMP 11 The mixture was added to the slurry in S2 and the mass ratio was controlled to be 4:1, and 5% Al2O3 was added. The mixture was mixed for 10 hours using a mixer to ensure the uniformity of the mixture.
[0143] S6. Place the mixed slurry in a glove box, use a coating machine to evenly coat the slurry on the copper tape using a scraper, and let it stand for 6 hours, so that a composite solid electrolyte membrane is formed on the copper tape.
[0144] Battery Assembly
[0145] Electrode preparation: The positive electrode material (NCM811) and the negative electrode material (lithium metal) are mixed evenly with the binder (PVDF), and coated on the positive electrode collector and the negative electrode collector to make the positive electrode and the negative electrode respectively.
[0146] Polymer electrolyte preparation: The polymer solid electrolyte film is prepared by the above method.
[0147] Battery assembly: The positive electrode, negative electrode and polymer electrolyte film are stacked together in sequence and then vacuum-sealed.
[0148] Performance Test:
[0149] The products obtained in the above examples and comparative examples were assembled: the membrane and the positive and negative electrode plates were assembled together in an inert gas glove box with a water and oxygen content of ≤0.01 ppm. The positive electrode had a NCM811 loading of 10 mg cm per unit area. -2 The electrode sheet, lithium metal as the negative electrode layer, and PVDF as the adhesive are assembled into a fully solid-state soft-pack lithium metal battery. Finally, the first efficiency is tested by cyclic discharge at 0.1C, and the capacity retention rate is tested after 50 cycles. The capacity retention rates of Example 1 and Comparative Example 1 are as follows: Figure 1 As shown, the results are shown in Table 1:
[0150] Table 1
[0151]
[0152] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for preparing a composite solid electrolyte membrane, characterized in that: The steps include: S1. Preparation of composite polymer electrolyte slurry: Adding the polymer to the solvent, adding the lithium salt, and stirring to obtain a uniform composite polymer electrolyte slurry; S2. Preparation of composite solid electrolyte membrane: Adding the co-solvent modified sulfide electrolyte mixture to the composite polymer electrolyte slurry, adding inorganic additives and mixing evenly to obtain a mixed slurry; coating the mixed slurry on a carrier, and drying to obtain the composite solid electrolyte membrane; In the mixed slurry of step S2, the mass proportions of the components used are: 50-80% of the co-solvent-modified sulfide electrolyte, 15-40% of the composite polymer electrolyte, and 5-10% of the inorganic additive; The co-solvent modified sulfide electrolyte is a co-solvent coated sulfide electrolyte; The co-solvent modified sulfide electrolyte is prepared by the following method: adding sulfide electrolyte powder to the co-solvent, uniformly dispersing the powder, sealing and standing for 10-24 hours, so that the co-solvent forms a coating layer on the surface of the sulfide electrolyte powder, and filtering out excess co-solvent to obtain the co-solvent modified sulfide electrolyte; The co-solvent includes one or more of N-methylpyrrolidone and dimethyl sulfoxide; the mass ratio of the co-solvent to the sulfide electrolyte powder is 2-3:7-8; The composite polymer electrolyte comprises a lithium salt and a polymer; The polymer includes two or more of polyethylene oxide, polycarbonate, polyvinylidene fluoride, polyacrylonitrile, polyethylene-propylene-butadiene rubber, sulfonated polyphenylene ether, polyethylene-ethylene oxide copolymer, polyethylene imine, and polyvinylidene fluoride-hexafluoropropylene; In the composite polymer electrolyte, the mass ratio of polymer to lithium salt is 2-3:1; the composite polymer electrolyte comprises at least two polymers, wherein the mass proportion of each polymer in the total amount of polymers is at least 10%.
2. The preparation method according to claim 1, characterized in that: The sulfide electrolyte is a crystalline sulfide electrolyte; the crystalline sulfide electrolyte includes one or more of Thio-LISICON type, LGPS type, and Argentum type.
3. The preparation method according to claim 1, characterized in that: The lithium salt includes one or a combination of lithium hexafluorophosphate, lithium chlorofluorosulfonate, lithium trifluoromethanesulfonate, lithium tetrafluoroborate, lithium perchlorate, lithium fluorosulfonate, lithium ethylenesulfonate, lithium trifluoroacetate, lithium tetrafluoroacetate, lithium pentafluoroacetate, and lithium bis(fluorosulfonyl)imide.
4. The preparation method according to claim 1, characterized in that: The inorganic additive is selected from one or more of SiO2 and Al2O3.
5. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of polymer, solvent and lithium salt is 2:1:1-3:3:1; And / or, the solvent includes one or more of ethylene glycol methyl ether, propylene glycol methyl ether, 1,3-dioxolane, triethyl phosphate, tetramethyl urea, ethyl trifluoromethanesulfonate, butyl tetrafluoroacetate, and propyl pentafluoroacetate.
6. Use of the composite solid electrolyte membrane obtained by the preparation method as claimed in claim 1 in the preparation of all-solid-state soft-pack batteries.
7. An all-solid-state soft-pack battery, characterized in that: The invention comprises a lithium metal negative electrode or a metal lithium composite negative electrode, a positive electrode and a composite solid electrolyte membrane obtained by the preparation method as claimed in claim 1.
Citation Information
Patent Citations
Composite electrolyte film for all-solid-state lithium metal negative electrode battery, preparation method of composite electrolyte film and all-solid-state sulfide lithium ion battery comprising composite electrolyte film
CN112599846A
High-flexibility sulfide composite solid electrolyte and preparation method thereof
CN112909332A