A method for preparing TC4ELI titanium alloy wire with excellent high-frequency fatigue strength

Through the specific titanium alloy wire composition and process flow, the problem of TC4ELI titanium alloy wire breaking under high-frequency vibration conditions has been solved, the high-frequency fatigue strength has been significantly improved, and the high-frequency fatigue performance requirements of medical ultrasonic scalpels have been met.

CN118543695BActive Publication Date: 2024-10-01BAOWU TEYE TITANIUM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027670.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-01
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

TC4ELI titanium alloy wire is prone to fracture under the high-frequency vibration conditions of medical ultrasonic scalpels, and existing technology cannot effectively improve its high-frequency fatigue strength and tissue uniformity.

Method used

Specific titanium alloy wire composition and process flow are adopted, including rounding and pre-drawing, hot drawing, cold drawing, heat treatment and straightening, to control the grain size and shape, and by gradually increasing the deformation amount and temperature treatment to ensure High frequency fatigue strength of wire.

Benefits of technology

The high-frequency fatigue strength of TC4ELI titanium alloy wire is significantly improved, the service life under high-frequency vibration conditions is extended, and the high-frequency fatigue performance requirements of medical ultrasonic scalpels are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118543695B_ABST
    Figure CN118543695B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a TC4ELI titanium alloy wire with excellent high-frequency fatigue strength, comprising the following steps of selecting a titanium alloy wire, wherein the titanium alloy wire is selected from a TC4ELI wire coil with a billet of φ10-14 mm, the organizational state is an α+β two-phase region equiaxed organization, the β grains are completely broken into granules, and the average α grain size is ≤12 μm; further comprising a rounding and pre-drawing stage, selecting less than or equal to 3 drawing passes, the deformation amount of a single pass needs to be gradually increased, and the cumulative deformation amount is less than or equal to 30%, to obtain a φ10±1 mm coil billet; further comprising a surface preparation stage; further comprising a hot drawing stage; further comprising a cold drawing stage; further comprising a heat treatment process. The TC4ELI titanium alloy wire obtained by the method of the present invention has excellent high-frequency fatigue strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metallurgy and relates to a method for manufacturing a metal material, in particular to a method for preparing a TC4ELI titanium alloy wire with excellent high-frequency fatigue strength. Background Art

[0002] TC4ELI titanium alloy is a titanium alloy obtained by reducing the fluctuation range of V and Al elements and reducing the maximum allowable content of light elements C, N, O and impurity elements on the basis of ordinary TC4 titanium alloy. TC4ELI titanium alloy has good damage tolerance performance and can be used as a high-quality aviation material or as a pressure-resistant medium shell, such as in manned submersibles. TC4ELI titanium alloy has a low content of impurity elements and excellent mechanical properties. It has always been the preferred material for surgical implants in the medical industry. At the same time, the titanium alloy wire obtained by continuous straightening is also very suitable for medical Kirschner wires.

[0003] In recent years, medical ultrasonic scalpels have been increasingly used in the field of medical surgery due to their excellent hemostatic performance and low damage to the human body. Their working mode requires the wire to have excellent high-frequency fatigue strength performance. In addition to the need to use TC4ELI titanium alloy with a lower content of impurity elements, the microstructure of the wire also needs to be controlled. It is generally believed that strength is related to the size of the grains in the organization. The smaller the grain size, the higher the strength; while fatigue performance is more related to the grain morphology, grain size and uniformity. This requires more stringent requirements on the manufacturing process.

[0004] GB / T 3623 Titanium and Titanium Alloy Wire Standard stipulates that the room temperature tensile strength of TC4ELI wire with a specification range of φ1~7mm is ≥860MPa, and the elongation after fracture is ≥10%; GB / T 13810 Titanium and Titanium Alloy Processing Materials for Surgical Implants stipulates that the room temperature tensile strength of TC4ELI wire with a specification range of φ1~7mm is ≥860MPa, the room temperature yield strength is ≥795MPa, and the elongation after fracture is ≥10%. In actual use, it is found that under the high-frequency vibration conditions of medical ultrasonic scalpels, even if the strength of TC4ELI wire meets the standard requirements, it will still break during use.

[0005] The patent for titanium and titanium alloy wire processing method (application publication number CN 101716715 A) discloses a titanium and titanium alloy processing method, which uses cold rolling to achieve the production of titanium and titanium alloy fine wires with a surface brightness of Φ1mm-Φ3mm and no oxidation. The characteristics are low cost and high efficiency, but the performance of the wire is not involved. At the same time, the cold-rolled wire generally has high strength and high dimensional accuracy but general plasticity. The patent for alloy processing technology and method for producing titanium rods and titanium wires (application publication number CN103192244 A) discloses the processing technology of titanium alloy wires. This method is a universal method for titanium wire production. The process includes electrode pressing, vacuum melting, forging and rolling. It also does not involve the structural uniformity and plasticity of the finished wire. Summary of the invention

[0006] In view of the above technical problems in the prior art, the present invention provides a method for preparing a TC4ELI titanium alloy wire with excellent high-frequency fatigue strength. The method for preparing a TC4ELI titanium alloy wire with excellent high-frequency fatigue strength is to solve the technical problem that the TC4ELI wire in the prior art is prone to breakage during long-term use under high-frequency vibration conditions.

[0007] The present invention provides a method for preparing a TC4ELI titanium alloy wire with excellent high-frequency fatigue strength, comprising the following steps:

[0008] 1) Select titanium alloy wire, the components of which are as follows:

[0009] Al 6.3±0.15wt%,

[0010] V 4.0±0.2wt%,

[0011] Fe ≤0.25wt%,

[0012] C ≤0.03wt%,

[0013] H ≤0.0008wt%,

[0014] O 0.12±0.1wt%,

[0015] N ≤0.01wt%,

[0016] Si ≤0.05wt%,

[0017] The balance is Ti and unavoidable impurities;

[0018] The titanium alloy wire material is selected from TC4ELI wire coils with a diameter of 10-14 mm, and the organizational state is a fully broken α+β two-phase region equiaxed organization, and the average α grain size is ≤12 μm;

[0019] 2) In the rounding and pre-drawing stage, select less than or equal to 3 drawing passes, the deformation of each pass needs to be gradually increased, the cumulative deformation is less than or equal to 30%, the deformation of the first drawing pass is ≤5%, but the maximum single-pass deformation is less than or equal to 15%, the heating temperature of the drawing blank is controlled at 880℃±20℃, the drawing line speed is controlled at 4-6m / min, and a Φ10±1mm round billet is obtained (Φ represents the diameter);

[0020] 3) In the surface preparation stage, the disc blank obtained in step 2) is subjected to centerless peeling and surface inspection. At this time, the size is Φ9.5±1mm (Φ represents the diameter), and there is no residual oxide scale or scarring on the surface;

[0021] 4) In the hot drawing stage, before drawing, the coil is first kept at 700~750℃ for 1h and then air-cooled to remove the stress of the previous process. The drawing temperature is controlled at 840~900℃, the total deformation is less than or equal to 70%, the deformation of the first pass is less than or equal to 8%, and the deformation gradually increases from the second pass. The maximum deformation of a single pass is less than or equal to 23%. It is divided into 3~5 drawing passes, and the drawing line speed is controlled at 2~4m / min;

[0022] 5) Cold drawing stage: Annealing treatment is used before drawing, and then cold drawing is carried out. During the cold drawing process, the deformation of each pass is less than or equal to 14%. Every 2 to 4 passes or when the cumulative deformation reaches 35%, it is kept at 700℃±50℃ for ≥1h and air-cooled. The total deformation should be ≤50%;

[0023] 6) Heat treatment process: The heat treatment is carried out in two stages. The first stage is carried out at 680±50℃ for 0.5~1h and air cooling, and then the second stage is carried out at 450±50℃ for 0.5~1h and air cooling to obtain TC4ELI titanium alloy wire with excellent high-frequency fatigue strength.

[0024] Preferably, the wire coil used for the titanium alloy wire is a hot-rolled product, because the continuous rolling method has higher deformation efficiency and more complete β-structure crushing.

[0025] Preferably, in the preparation process of step 6), a vacuum heat treatment method is selected to effectively further reduce the H content of the finished wire material.

[0026] Furthermore, after the first stage heat treatment in step 6) is completed, cold straightening is performed, and after straightening, a second stage heat treatment and air cooling are performed.

[0027] Preferably, the post-processing method of the titanium alloy wire is mainly straightening, heat treatment and polishing, which specifically includes the following steps:

[0028] Step 1: Use a multi-roller cold straightening machine to straighten the wire coil after drawing;

[0029] Step 2: Cut to length according to 1~3m;

[0030] Step 3: Roughly grind to the specified size;

[0031] Step 4: Heat treatment according to 450±50℃ / 0.5~1h air cooling process;

[0032] Step 5: Fine grinding to the specified size, the specific tolerance is carried out according to product standards or user requirements.

[0033] Compared with the prior art, the technical effect of the present invention is positive and obvious. The TC4ELI titanium alloy wire obtained by the preparation method of the present invention has excellent high-frequency fatigue strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a high-magnification structure of φ12mm TC4ELI wire coil.

[0035] Figure 2 It is the φ5.5mmTC4ELI wire structure.

[0036] Figure 3 The EBSD contrast image (left) and grain boundary distribution image (right) of the φ5.5mm TC4ELI wire coil.

[0037] Figure 4 High frequency fatigue test results. DETAILED DESCRIPTION

[0038] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0039] Example

[0040] Step 1: Select TC4ELI titanium alloy wire coil with Al 6.2wt%, V 3.85wt%, Fe 0.03wt%, C0.01wt%, H 0.0006wt%, O 0.13wt%, N 0.003wt% and Si 0.01wt%, and the balance is Ti and unavoidable impurities.

[0041] Select φ12mmTC4ELI wire coil, its structure is as shown in the attached Figure 1As shown, it is a uniformly distributed α+β two-phase region structure, in which the β phase has been completely broken into particles, and the average α grain size is about 3 to 10 μm.

[0042] Step 2: Round and pre-draw the coil according to the process shown in the table below;

[0043] In this stage, the roundness of the cross section of the coil needs to be improved, so the deformation of each pass needs to be gradually increased, but not more than 3 drawing passes, and the deformation does not exceed 30%. The deformation of the first drawing pass is ≤5%, and the deformation of the second and third drawing passes should be higher than the first drawing pass, but the maximum single-pass deformation does not exceed 15%. The heating temperature of the drawing blank is controlled at 880℃±20℃, and the drawing line speed can be appropriately increased to improve production efficiency, controlled at 4-6m / min. Finally, a Φ10±1mm coil blank is obtained from this step.

[0044] The specific process of step 2 is shown in Table 1:

[0045] Table 1

[0046]

[0047] Heat treatment and hot drawing are carried out according to the process shown in the table below.

[0048] Step 3: It also includes a surface preparation stage. In this stage, the coil blank prepared in the previous step is subjected to centerless peeling and surface inspection. At this time, the size is Φ9.5±1mm, and there are no defects such as oxide scale residue and scars visible to the naked eye on the surface.

[0049] Step 4: It also includes a hot drawing stage: This stage mainly homogenizes the grain size through a more appropriate deformation amount. Before drawing, the disc is first heat treated at 720℃ for 1h and air-cooled to remove the stress of the previous process. The drawing temperature is controlled at 840~900℃, the total deformation does not exceed 70%, the first deformation does not exceed 8%, and the lubricant is better covered on the surface. The deformation is gradually increased from the second pass, and the maximum deformation of a single pass does not exceed 23%. It can be divided into 3~5 drawing passes. The drawing line speed is controlled at 2~4m / min.

[0050] The specific process of step 4 is shown in Table 2:

[0051] Table 2

[0052]

[0053] Annealing, cold drawing and first heat treatment are carried out according to the process shown in the table below.

[0054] Step 5: Cold drawing stage: This stage mainly involves continuous cold deformation to deform the α grain boundary, changing it from an equiaxed distribution to a mutually rolling shape, and accumulating deformation storage energy at the same time. However, if the cumulative deformation during cold deformation is too large, resulting in too high deformation storage energy, the grain recovery will be too sufficient during the subsequent annealing process, which is seriously unfavorable to improve fatigue strength. Therefore, the deformation amount per pass in this stage does not exceed 14%, and every 2 to 4 passes or when the cumulative deformation reaches 35%, a heat treatment of 700℃±50℃ for ≥1h and air cooling should be carried out, and the total deformation should be ≤50%. Annealing process is used before drawing.

[0055] Step 6: Heat treatment: After the above cold drawing steps, the wire material now forms mutually rolling α grains with an average grain size of 1~6μm. The transformed β structure has formed fine dispersed particles distributed in the matrix, and there are a certain number of point defects. In order to promote the nucleation of grains in the point defects, heat treatment is required to improve plasticity. However, the heat treatment time should not be too long or the temperature should not be too high, otherwise the grains are prone to over-recovery, thereby increasing the average grain size and equiaxed grains, causing fatigue strength to decrease.

[0056] The heat treatment is carried out in two stages. The first stage is to keep the temperature at 680±50℃ for 0.5~1h and air cool. If there are requirements for the shape of the wire itself, cold straightening can be carried out after this step.

[0057] After straightening, the second stage is carried out at 450±50℃ / 0.5~1h and air cooling.

[0058] The specific process of steps five and six is ​​shown in Table 3:

[0059] Table 3

[0060]

[0061] The microstructure of the finished TC4ELI wire made by the above process is as follows: Figure 3 As shown, it is a uniformly distributed α+β structure, in which the transformation β is distributed in the matrix in a granular form, such as Figure 2 shown.

[0062] Since the wire structure is too fine at this time, EBSD analysis technology is used to analyze the structure, such as Figure 3 As shown. It can be seen that the α grain morphology in the current wire structure is mainly composed of wedge-shaped, kinked and small-particle equiaxed grains. According to the results of statistical calculations, the average grain size is 1.637 microns and the standard deviation σ of the grain size is 0.66μm.

[0063] The mechanical properties of the finished TC4ELI wire obtained by the above step six process (corresponding to two groups of parallel samples with the same preparation process) are shown in Table 4.

[0064] Table 4

[0065]

[0066] The wire produced by the above process and other typical domestic and imported wires are used to make the ultrasonic knife bar with the same vibration frequency, and the amplitude is selected in the range of 75~105μm. It vibrates until it breaks. The longer the time, the higher the high-frequency fatigue strength performance. The final conclusion is as follows Figure 4 As shown in the figure. The horizontal axis is the amplitude and the vertical axis is the logarithmic coordinate of the break time.

[0067] In addition, since the wire produced by this process did not break for too long under the conditions of 75 and 80 μm amplitudes, and did not break for more than 144 hours, only the test results of 85-105 μm were given. 100 and 105 μm are not the commonly used amplitude ranges of general ultrasonic surgical knives. Here, since the high-frequency fatigue strength of the material in this embodiment is good, additional tests were added, so no tests were performed on other materials.

[0068] Table 5 is a comparison of the standard composition of TC4ELI for implantable medical devices and the composition of imported and designed materials of the present invention (the balance is Ti and unavoidable impurities).

[0069] Table 5

[0070]

[0071] From the perspective of composition, the material of the present invention has two significant differences in composition design compared to imported materials. The first is that the content of impurity element Fe is much lower than that of imported material 1, and the composition of interstitial element O is closer to the standard upper limit.

[0072] from Figure 4 It can be seen that under the condition of 85μm, the high-frequency fatigue performance test results of this process are at the same level as those of imported materials, but under the condition of high amplitude, the high-frequency fatigue performance of the wire material of this process comprehensively surpasses the imported wire material.

[0073] High-frequency fatigue test method: The raw materials are processed into the same blade shape and loaded into the same ultrasonic knife. The ultrasonic knife has a transducer and is equipped with the same control system, and finally the vibration frequency of the blade head reaches 55kHz. After setting different amplitudes, it is repeatedly cut on the animal tissue until it breaks.

Claims

1. A method for preparing TC4ELI titanium alloy wire with excellent high-frequency fatigue strength, Features The steps include: 1) Select titanium alloy wire, the components of which are as follows: Al 6.3±0.15wt%, V 4.0±0.2wt%, Fe ≤0.25wt%, C ≤0.03wt%, H ≤0.0008wt%, O 0.12±0.1wt%, N ≤0.01 wt %, Si ≤0.05wt%, The balance is Ti and unavoidable impurities; The titanium alloy wire material is selected from TC4ELI wire coils with a diameter of 10-14 mm, the organizational state is an equiaxed organization in the α+β two-phase region, the β grains are completely broken into granules, and the average α grain size is ≤12 μm; 2) In the rounding and pre-drawing stage, select less than or equal to 3 drawing passes, the deformation of each pass needs to be gradually increased, the cumulative deformation is less than or equal to 30%, the deformation of the first drawing pass is ≤5%, but the maximum single-pass deformation is less than or equal to 15%, the heating temperature of the drawing blank is controlled at 880℃±20℃, and the drawing line speed is controlled at 4-6m / min to obtain a Φ10±1mm round billet; 3) In the surface preparation stage, the round disc obtained in step 2) is subjected to centerless peeling and surface inspection. At this time, the size is Φ9.5±1mm, and there is no residual oxide scale or scarring on the surface; 4) In the hot drawing stage, the coil is first kept at 700-750℃ for 1h before drawing, and then air-cooled to remove the stress of the previous process. The drawing temperature is controlled at 840-900℃, the total deformation is less than or equal to 70%, the deformation of the first pass is less than or equal to 8%, and the deformation gradually increases from the second pass. The maximum deformation of a single pass is less than or equal to 23%. It is divided into 3-5 drawing passes, and the drawing line speed is controlled at 2-4m / min; 5) Cold drawing stage: Annealing process is used before drawing, and then cold drawing is carried out. During the cold drawing process, the deformation of each pass is less than or equal to 14%. When the cumulative deformation reaches 35%, it is kept at 700℃±50℃ for ≥1h and air-cooled every 2~4 passes. The total deformation should be ≤50%; 6) Heat treatment process: The heat treatment is carried out in two stages. The first stage is carried out at 680±50℃ for 0.5~1h and air cooling, and then the second stage is carried out at 450±50℃ for 0.5~1h and air cooling to obtain TC4ELI titanium alloy wire with excellent high-frequency fatigue strength.

2. The method for preparing a TC4ELI titanium alloy wire having excellent high-frequency fatigue strength according to claim 1, Features: In the preparation process of step 6), a vacuum heat treatment method is selected.

3. The method for preparing a TC4ELI titanium alloy wire having excellent high-frequency fatigue strength according to claim 1, Features: After the first stage heat treatment in step 6), cold straightening is performed, and after cold straightening, the second stage heat treatment and air cooling are performed.