A method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material and a battery
Through positively charged colloid preparation and spray drying technology, anionic surfactants are used to adjust the carbon source distribution, which solves the problem of carbon sources gathering on the surface of droplets, achieves uniform carbon coating of lithium iron phosphate cathode materials, and improves the energy of the battery. Density and electrical properties.
Patent Information
- Application Number
- CN202411023975.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-29
AI Technical Summary
In the existing preparation methods of lithium iron phosphate cathode materials, carbon sources tend to accumulate on the surface of droplets, resulting in uneven carbon coating and affecting the high energy density and electrical performance of the battery.
Positively charged colloid preparation, prefabricated slurry preparation and spray drying technology are used to adjust the carbon source distribution through anionic surfactants to form a uniform carbon source coated lithium iron phosphate material to prevent the carbon source from gathering on the surface of the droplets during the spray drying process. , ensuring uniform coating of the carbon layer.
It achieves uniform distribution of carbon sources and regular agglomeration growth of lithium iron phosphate materials, improves the energy density and cycle life of the battery, avoids the formation of floating carbon, and improves the electrical performance of the battery.
Smart Images

Figure CN118545693B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy batteries, and in particular to a method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material and a battery. Background Art
[0002] As the world pays more and more attention to renewable energy and environmental protection technology, lithium-ion batteries, as an efficient and environmentally friendly energy storage device, have received widespread attention. In lithium-ion batteries, the positive electrode material is one of the key factors that determine its performance. Lithium iron phosphate positive electrode material has become a hot topic of current research due to its advantages such as high safety, high energy density, long cycle life and low cost.
[0003] In order to further improve the performance of lithium iron phosphate cathode materials, researchers have improved their conductivity, energy density, cycle life and other properties through modification techniques such as doping and coating. For example, hydrochloric acid treatment, carbon black conductive agent modification, graphene coating and other methods can effectively improve the conductivity of lithium iron phosphate cathode materials, thereby improving the discharge performance and cycle life of the battery.
[0004] The current mainstream route for the industrialization of lithium iron phosphate is to use iron phosphate + lithium carbonate + water-soluble carbon source (glucose, sucrose) as the raw material system, and form carbon-coated lithium iron phosphate through spray drying and high-temperature solid-phase reaction.
[0005] However, the existing preparation methods have many shortcomings, such as:
[0006] The carbon source tends to gather on the surface and is unevenly distributed, which reduces the carbon coating effect of the internal particles and leads to poor electrical performance. During the spray drying process, the water-soluble carbon source tends to move to the surface of the droplets, and the nanoparticles tend to remain inside the droplets, causing the water-soluble carbon source to gather on the surface, resulting in a lack of carbon source in the internal particles, reducing the carbon coating effect. On the other hand, the carbon source has the function of isolating the agglomeration growth of the precursor particles. The internal particles lack the carbon source and tend to grow irregularly, resulting in large particles of lithium iron phosphate with poor conductivity.
[0007] Carbon sources tend to accumulate on the surface. Too much carbon source on the surface will cause excess carbon, and the uncoated carbon will form floating carbon, resulting in low compaction density of the product, which is not conducive to achieving high energy density lithium iron phosphate batteries. Summary of the invention
[0008] The purpose of the present invention is to provide a method for uniformly carbon-coated lithium iron phosphate positive electrode material to solve the problem in the prior art that during spray drying, the carbon source is easily aggregated on the surface of the droplets to form a large amount of floating carbon, which affects the carbon coating and is not conducive to achieving a high energy density lithium iron phosphate battery.
[0009] In order to solve the above problems, the present invention adopts the following technical means:
[0010] A method for uniformly carbon-coated lithium iron phosphate positive electrode material, comprising:
[0011] Preparation of positively charged colloids: Preparation of Fe-containing colloids by mixing soluble iron sources with insoluble iron sources 2+ Positively charged colloid A;
[0012] Preparation of prefabricated slurry: adding a lithium source, a phosphorus source, a carbon source with a negatively charged group and an anionic surfactant to colloid A, mixing and ball milling to obtain a prefabricated slurry;
[0013] Precursor preparation: spray drying the prefabricated slurry to form a precursor uniformly coated with carbon source;
[0014] Molding: The precursor is sintered and molded to obtain a lithium iron phosphate material with a carbon source uniformly coated thereon.
[0015] More optimally, the preparation of the positively charged colloid comprises the following steps:
[0016] Preparation of soluble iron source solution: Mix ferrous sulfate as an iron source with deionized water at a ratio of 5:1 to obtain a soluble iron source solution containing Fe. 2+ Aqueous solution A;
[0017] Preparation of insoluble iron source colloid: mixing iron hydroxide or iron oxide as an insoluble iron source with deionized water in a ratio of 1:1, grinding in a sand mill to prepare an iron-containing colloid;
[0018] The aqueous solution A is mixed with the iron-containing colloid and dispersed to obtain a Fe-containing colloid. 2+ Positively charged colloid A.
[0019] Furthermore, in the iron-containing colloid, the particle size is 20-100 nm.
[0020] Furthermore, the lithium source is one of lithium carbonate, lithium hydroxide, lithium phosphate, and lithium dihydrogen phosphate.
[0021] Furthermore, the phosphorus source is one of phosphoric acid, diammonium hydrogen phosphate, monoammonium phosphate, and triammonium phosphate.
[0022] Furthermore, the anionic surfactant is one of N-acylaminocarboxylic acid, diethyl malonate, methyl methacrylate, maleic anhydride, and ammonium dodecyl diphenyl oxide disulfonate, and the added amount is 0.1wt%~5wt% of the soluble iron source.
[0023] Furthermore, in the precursor preparation process, the atomizer for spray drying is an ultrasonic atomizer, the inlet temperature is 200-270°C, and the outlet temperature is 100-110°C.
[0024] Furthermore, during the molding process, the precursor is placed in an inert atmosphere at 600-800° C. for 6-14 hours.
[0025] In addition, a lithium iron phosphate battery is made of the aforementioned lithium iron phosphate positive electrode material.
[0026] During use, the present invention has the following beneficial effects:
[0027] By selecting a material system in which the electric charge of the iron source / phosphorus source is opposite to that of the carbon source, the water-soluble carbon source can be reduced from moving to the liquid surface and aggregating during spray drying and granulation. This makes the carbon source and the iron source / phosphorus source evenly distributed, making it easier to react and generate lithium iron phosphate materials with uniform particle size, regular morphology, and uniform carbon coating.
[0028] During spray drying, the negatively charged characteristics of anionic surfactants are utilized to facilitate the adsorption of carbon sources near the positively charged iron sources during the spray drying process, thereby preventing the carbon sources from moving to the droplet surface and aggregating; and the carbon sources can slowly form a carbon layer during spray drying, which is more conducive to the uniformity of carbon coating. This prevents the carbon layer from forming under the conditions of rapid temperature rise during high-temperature solid-phase sintering, and the carbon source from violently decomposing into carbon, resulting in poor coating effects.
[0029] At the same time, the positively charged iron source / phosphorus source and the negatively charged carbon source react in the iron source colloid system, and the particle sizes are close. During the spray drying process, the movement rates of the components are the same, and lithium iron phosphate precursor particles with uniform structural distribution can be obtained. After sintering, the product has good uniformity and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 TEM image of the lithium iron phosphate positive electrode material provided in Example 1 of the present invention.
[0031] Figure 2 This is the XRD diagram of the lithium iron phosphate positive electrode material provided in Example 1 of the present invention.
[0032] Figure 3 CV curves of the lithium iron phosphate positive electrode materials provided in Example 1 of the present invention and Comparative Example 1.
[0033] Figure 4 This is a low temperature rate performance diagram of the lithium iron phosphate positive electrode material provided in Example 1 of the present invention and Comparative Example 1.
[0034] Figure 5 This is a 1C cycle performance diagram of the lithium iron phosphate positive electrode material provided in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0036] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.
[0038] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0039] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the product of the invention is usually placed when in use, or the positions or positional relationships commonly understood by those skilled in the art, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0040] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0041] A method for uniformly carbon-coated lithium iron phosphate positive electrode material, comprising:
[0042] Preparation of positively charged colloids: Preparation of Fe-containing colloids by mixing soluble iron sources with insoluble iron sources 2+ Positively charged colloid A.
[0043] Among them, a double iron source is used to form a Fe 2+ The positively charged colloid A avoids the introduction of impurities that would affect the purity of the finished lithium iron phosphate.
[0044] Preparation of prefabricated slurry: lithium source, phosphorus source, anionic surfactant (carbon source with negatively charged groups) are added to colloid A, mixed and then ball-milled to obtain prefabricated slurry.
[0045] In this way, anionic surfactants with prominent negative charge characteristics are used, and the raw materials are controlled and mixed by ball milling, so that the negatively charged carbon source surrounds the Fe 2+ The positively charged colloid A aggregates around the particles for subsequent spray drying.
[0046] Precursor preparation: The prefabricated slurry is spray-dried to form a precursor uniformly coated with a carbon source.
[0047] When the prepared prefabricated slurry is spray-dried, the iron source is positively charged and the carbon source is negatively charged, and the Fe 2+ The characteristics of the spray drying agent can be used to inhibit the decomposition and carbonization of carbon and prevent the carbon source from moving to the droplet surface and gathering during the spray drying process, effectively avoiding the formation of floating carbon. In this way, the carbon layer can be slowly formed during spray drying, which is conducive to the uniform coating of the carbon layer.
[0048] Molding: The precursor is sintered and molded to obtain a lithium iron phosphate material with a carbon source uniformly coated thereon.
[0049] Preferably, the preparation of the positively charged colloid comprises the following steps:
[0050] Preparation of soluble iron source solution: Mix ferrous sulfate as an iron source with deionized water at a ratio of 5:1 to obtain a soluble iron source solution containing Fe. 2+ Aqueous solution A;
[0051] Preparation of insoluble iron source colloid: mixing iron hydroxide or iron oxide as an insoluble iron source with deionized water in a ratio of 1:1, grinding in a sand mill to prepare an iron-containing colloid;
[0052] The aqueous solution A is mixed with the iron-containing colloid and dispersed to obtain a Fe-containing colloid. 2+ Positively charged colloid A.
[0053] The molar ratio of iron source to phosphorus source of lithium iron phosphate is Fe:P=0.90~1:1. If the Fe source is added too little, the lithium iron phosphate will be unstable due to lack of iron, resulting in performance degradation. If the Fe source is added too much, iron-containing impurities are easily generated, affecting the thermal stability of the lithium iron phosphate battery.
[0054] In the aforementioned iron-containing colloid, the particle size is 20~100nm.
[0055] Preferably, the aforementioned lithium source is one of lithium carbonate, lithium hydroxide, lithium phosphate, and lithium dihydrogen phosphate.
[0056] Preferably, the phosphorus source is one of phosphoric acid, diammonium hydrogen phosphate, monoammonium phosphate, and triammonium phosphate.
[0057] At the same time, the aforementioned anionic surfactant is one of N-acylaminocarboxylic acid, diethyl malonate, methyl methacrylate, maleic anhydride, and ammonium dodecyl diphenyl ether disulfonate. The added amount is 0.1wt%~5wt% of the soluble iron source. If the carbon source is added too little, the effect of uniform carbon coating cannot be achieved. If the carbon source is added too much, floating carbon is easily caused, which affects the compaction density of the lithium iron phosphate positive electrode material, which is not conducive to the preparation of a high energy density lithium iron phosphate battery.
[0058] Furthermore, in the precursor preparation process, the atomizer for spray drying is an ultrasonic atomizer, the inlet temperature is 200-270°C, and the outlet temperature is 100-110°C.
[0059] Furthermore, during the spray drying process, on the one hand, an ultrasonic atomizer is used to utilize ultrasound to promote the agglomeration of positive and negative charges in the early stage of spray drying to form uniform spherical droplet particles, while preventing the water-soluble carbon source from moving toward the liquid surface, thereby making the carbon source and the iron source evenly distributed.
[0060] In addition, the negatively charged groups of anionic surfactants are advantageously adsorbed near the positively charged iron source, so that a carbon layer is slowly formed during spray drying, while preventing carbon from decomposing / carbonizing too quickly to form floating carbon.
[0061] Furthermore, during the molding process, the precursor is placed in an inert atmosphere at 600-800° C. for 6-14 hours.
[0062] In addition, a lithium iron phosphate battery is made of the aforementioned lithium iron phosphate positive electrode material.
[0063] The following is a further description with reference to specific preparation examples.
[0064] Example 1
[0065] S1. Mix ferrous sulfate and deionized water in a mass ratio of 5:1 and dissolve to obtain a Fe-containing 2+ of aqueous solution A.
[0066] S2. Place ferric hydroxide or ferric oxide and deionized water in a sand mill at a mass ratio of 1:1 and grind for 4 to 6 hours with a grinding medium diameter of 0.15 mm and a rotation speed of 1000 to 3000 rad / min to obtain an iron-containing colloid with a particle size of 20 to 100 nm.
[0067] S3. Mix the aqueous solution A with the iron-containing colloid and disperse for 30 to 60 minutes to obtain a Fe-containing colloid. 2+ Positively charged colloid A.
[0068] S4. Add lithium phosphate to colloid A, wherein the lithium phosphate is used as both a phosphorus source and a lithium source, and the molar ratio of Fe:P is 0.9-1; the molar ratio of Li:Fe is 1-1.04, and then add N-acylaminocarboxylic acid or diethyl malonate or methyl methacrylate or maleic anhydride or ammonium dodecyl diphenyl ether disulfonate as an anionic surfactant, and the added amount is 0.1%-5% of the mass fraction of ferrous sulfate and ferric oxide / ferric hydroxide;
[0069] After mixing, place it in a ball mill with a speed of 800~1500rad / min, a ball milling time of 4~8h, and a ball size of 0.2mm~1mm, and grind the slurry to a particle size of 100~200nm.
[0070] S5. The slurry is spray-dried, the atomizer is an ultrasonic atomizer, the inlet temperature is 200-270° C., and the outlet temperature is 100-110° C., thereby forming a lithium iron phosphate precursor uniformly coated with a carbon source.
[0071] S6. The aforementioned lithium iron phosphate precursor is placed in an inert atmosphere for sintering at 600-800° C. for 6-14 hours to form a spherical lithium iron phosphate material uniformly coated with carbon.
[0072] Example 2
[0073] S1. Mix ferrous sulfate and deionized water in a mass ratio of 5:1 and dissolve to obtain a Fe-containing 2+ of aqueous solution A.
[0074] S2. Place ferric hydroxide or ferric oxide and deionized water in a sand mill at a mass ratio of 1:1 and grind for 4 to 6 hours with a grinding medium diameter of 0.15 mm and a rotation speed of 1000 to 3000 rad / min to obtain an iron-containing colloid with a particle size of 20 to 100 nm.
[0075] S3. Mix the aqueous solution A with the iron-containing colloid and disperse for 30 to 60 minutes to obtain a Fe-containing colloid.2+ Positively charged colloid A.
[0076] S4. Add lithium phosphate and phosphoric acid to colloid A, so that the molar ratio of Fe:P is 0.9-1; the molar ratio of Li:Fe is 1-1.04, and then add N-acylaminocarboxylic acid or diethyl malonate or methyl methacrylate or maleic anhydride or ammonium dodecyl diphenyl ether disulfonate as an anionic surfactant, and the added amount is 0.1%-5% of the mass fraction of ferrous sulfate and ferric oxide / ferric hydroxide;
[0077] After mixing, place it in a ball mill with a speed of 800~1500rad / min, a ball milling time of 4~8h, and a ball size of 0.2mm~1mm, and grind the slurry to a particle size of 100~200nm.
[0078] S5. The slurry is spray-dried, the atomizer is an ultrasonic atomizer, the inlet temperature is 200-270° C., and the outlet temperature is 100-110° C., thereby forming a lithium iron phosphate precursor uniformly coated with a carbon source.
[0079] S6. The aforementioned lithium iron phosphate precursor is placed in an inert atmosphere for sintering at 600-800° C. for 6-14 hours to form a spherical lithium iron phosphate material uniformly coated with carbon.
[0080] Comparative Example 1
[0081] S1. The ferrous sulfate, lithium phosphate, mixed, mixed with sodium citrate or sodium oxalate, adding anionic surfactant;
[0082] After mixing, place in a ball mill and ball-mill to a particle size of 100-200 nm.
[0083] S2. The slurry formed in S1 is spray dried, the atomizer is an ultrasonic atomizer, the inlet temperature is 200-270° C., and the outlet temperature is 100-110° C., thereby forming a lithium iron phosphate precursor uniformly coated with a carbon source.
[0084] S3. The aforementioned lithium iron phosphate precursor is placed in an inert atmosphere for sintering at 600-800° C. for 6-14 hours to form a lithium iron phosphate material.
[0085] Experimental Example 1
[0086] Figure 1 This is the TEM spectrum of the lithium iron phosphate material prepared in Example 1 of the present invention, which shows that carbon is indeed evenly distributed around the lithium iron phosphate particles, and there is also carbon inside the particles, and it is not accumulated on the surface of the particles during the spray drying process. The problem of a large amount of floating carbon being easily generated in the existing production process is solved.
[0087] Experimental Example 2
[0088] The lithium iron phosphate material prepared in Example 1 was tested by XRD and compared with the standard card, indicating that pure phase lithium iron phosphate can be generated without impurities. Figure 2 shown.
[0089] Experimental Example 3
[0090] The discharge gram capacity of Example 1 is compared with that of Comparative Example 1. The discharge gram capacity of Example 1 at 0.1C under a charge and discharge voltage of 2-3.75V is 162mAh / g; the discharge gram capacity of Comparative Example 1 at 0.1C under a charge and discharge voltage of 2-3.75V is 156mAh / g. Figure 3 shown.
[0091] Experimental Example 4
[0092] The low temperature rate performance test was carried out on Example 1 and Comparative Example 1. At -20°C and 2-3.75V charge and discharge voltage, the 5C / 1C capacity retention rate of Example 1 was 88%, while that of Comparative Example 1 was 80%, indicating that the uniformly coated lithium iron phosphate material involved in the present application can effectively improve the low temperature rate performance. Figure 4 shown.
[0093] Experimental Example 5
[0094] The cycle life test of Example 1 and Comparative Example 1 was conducted, and the charge and discharge voltage was 2-3.75V at room temperature, and the charge and discharge current was 1C for 100 cycles. The retention rate of Example 1 was 98.6%. The retention rate of Comparative Example 1 was 91.2%. Figure 5 shown.
[0095] For the aforementioned test structure, since the lithium iron phosphate material prepared in Comparative Example 1 is difficult to form a preliminary carbon coating during the spray drying process, the carbon cannot be evenly coated on the base particles due to the violent reaction during the sintering process. At the same time, during the spray drying process of Comparative Example 1, a large amount of carbon floats on the surface of the droplets, and a large amount of floating carbon is formed after drying, making it difficult to form a carbon film coating the base particles. Therefore, the electrical properties of Comparative Example 1 are inferior to those of the lithium iron phosphate material prepared in Example 1.
[0096] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material, characterized in that: include: Preparation of positively charged colloids: Preparation of Fe-containing colloids by mixing soluble iron sources with insoluble iron sources 2+ Positively charged colloid A; Preparation of prefabricated slurry: adding a lithium source, a phosphorus source, and an anionic surfactant as a carbon source to colloid A, mixing and ball milling to obtain a prefabricated slurry; Precursor preparation: spray drying the prefabricated slurry to form a precursor uniformly coated with carbon source; Molding: The precursor is sintered and molded to obtain a lithium iron phosphate material with a carbon source uniformly coated thereon.
2. The method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material according to claim 1, characterized in that: The positive charge colloid preparation comprises the following steps: Preparation of soluble iron source solution: Mix ferrous sulfate as an iron source with deionized water at a ratio of 5:1 to obtain a soluble iron source solution containing Fe. 2+ Aqueous solution A; Preparation of insoluble iron source colloid: mixing iron hydroxide or iron oxide as an insoluble iron source with deionized water in a ratio of 1:1, grinding in a sand mill to prepare an iron-containing colloid; The aqueous solution A is mixed with the iron-containing colloid and dispersed to obtain a Fe-containing colloid. 2+ Positively charged colloid A.
3. The method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material according to claim 2, characterized in that: In the iron-containing colloid, the particle size is 20-100 nm.
4. The method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material according to claim 1, characterized in that: The lithium source is one of lithium carbonate, lithium hydroxide, lithium phosphate and lithium dihydrogen phosphate.
5. The method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material according to claim 1, characterized in that: The phosphorus source is one of lithium phosphate, phosphoric acid, diammonium hydrogen phosphate, monoammonium phosphate and triammonium phosphate.
6. The method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material according to claim 1, characterized in that: The anionic surfactant is one of N-acylaminocarboxylic acid, diethyl malonate, methyl methacrylate, maleic anhydride, and ammonium dodecyl diphenyl oxide disulfonate, and the added amount is 0.1wt% to 5wt% of the soluble iron source.
7. The method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the precursor preparation process, the atomizer for spray drying is an ultrasonic atomizer, the inlet temperature is 200-270°C, and the outlet temperature is 100-110°C.
8. The method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material according to claim 1, characterized in that: During the molding process, the precursor is placed in an inert atmosphere at 600-800° C. for 6-14 hours.
9. A battery, characterized in that: The positive electrode material used is a lithium iron phosphate material prepared by the method for preparing a uniformly carbon-coated lithium iron phosphate positive electrode material according to any one of claims 1 to 8.