Colored flashing dry particles, colorful glare ceramic tiles and preparation method thereof
By using the combination of burn-free colored dry particles and zircon sand dry particles, the problem of the emulsion of zircon sand dry particles affecting the inkjet pattern is solved, the scope of use of zircon sand is broadened and the multiple visual effects of color and flash are achieved , improves the glaze quality and anti-fouling performance of ceramic products.
Patent Information
- Application Number
- CN202411019037.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing flash ceramic products have affected the color of the inkjet pattern due to the emulsion of the dry particles of zircon sand, resulting in poor matching between the ceramic products and the layout design, limiting the scope of use of zircon sand.
Colored flash dry particles composed of flammable colored dry particles and zircon sand dry particles are used. The colored flash dry particles are pelletized by spray drying, combined with inkjet printing and application methods of transparent dry particles glaze to achieve multiple visual effects of color and flash.
The scope of use of zircon sand dry particles has been broadened, the influence of zircon sand dry particles on the ink pattern is avoided, the glaze quality and anti-fouling performance of ceramic products has been improved, and multiple visual effects of color and flash are achieved.
Smart Images

Figure CN118545909B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to colored flashing dry particles, colorful glare ceramic tiles and a preparation method thereof, belonging to the technical field of ceramic tile production and manufacturing. Background Art
[0002] With the improvement of living standards, people's requirements for home decoration are gradually developing in the direction of personalization, and the requirements for the surface texture of ceramic products are also getting higher and higher. In recent years, glittering ceramic products have been favored by consumers. For example, building ceramic companies have proposed adding zircon sand to polishing glaze or dry granular glaze to make glittering glaze, and then applying the glittering glaze to the surface of the body, firing and polishing to obtain ceramic products with glittering effects. Since natural zircon sand itself has opacity, when zircon sand dry particles are distributed on the surface of the body over a large area, the color of the inkjet pattern layer located under the zircon sand dry particle layer will be affected, which ultimately leads to poor matching between the ceramic product and the layout design. In order to avoid this situation, building ceramic companies can usually only distribute large areas of zircon sand in the corresponding positions of the white pattern, but this has caused limitations in product pattern design to a certain extent. Summary of the invention
[0003] In response to the problems raised by the background technology, the present invention provides a colored glittering dry particle, a colored glare ceramic tile and a preparation method thereof. By using the colored glittering dry particle composed of unfired colored dry particles and zircon sand dry particles, the influence of the opacity of the zircon sand dry particles themselves on the ink pattern decoration is avoided, the application scope of zircon sand is broadened, and multiple visual effects of color and glitter are achieved.
[0004] In a first aspect, the present invention provides a colored flashing dry granule. The raw material composition of the colored flashing dry granule includes: by mass percentage, 20-50% of unburned colored dry granule and 50-80% of zircon sand dry granule. The unburned colored dry granule includes basic minerals and colorants; wherein the chemical composition of the basic minerals of the unburned colored dry granule includes: by mass percentage, SiO2: 60-70%; Al2O3: 18-26%; Fe2O3: 0.1-0.3%; TiO2: 0.1-0.2%; MgO: 0.1-0.3%; CaO: 0.1-0.4%; K2O: 1-5%; Na2O: 4-6%; ignition loss: 2-5%.
[0005] Preferably, the raw material composition of the basic minerals of the unburned colored dry particles includes, by mass percentage, 5-40% potassium feldspar, 25-55% sodium feldspar, 20-45% kaolin, and 5-10% quartz powder.
[0006] Preferably, the particle size of the unburned colored dry particles is 60-100 mesh; the particle size of the zircon sand dry particles is 60-100 mesh.
[0007] Preferably, the method for preparing the unfired colored dry granules comprises: weighing each raw material according to the raw material composition of the basic minerals of the unfired colored dry granules, adding water and an auxiliary agent, and mixing them evenly to prepare a basic glaze slurry of the unfired colored dry granules; then adding a colorant to the basic glaze slurry of the unfired colored dry granules, mixing them evenly again, and preparing a glaze slurry of the unfired colored dry granules; spray drying and granulating the unfired colored dry granules glaze slurry to obtain unfired colored dry granules. Preferably, the auxiliary agent comprises sodium tripolyphosphate and sodium carboxymethyl cellulose.
[0008] In a second aspect, the present invention provides a method for preparing a colored glare ceramic tile. The preparation method comprises the following steps:
[0009] Applying glaze on the surface of the body;
[0010] Inkjet printing a common ink pattern on the surface of the body after the glaze is applied;
[0011] Inkjet printing a glue pattern on the surface of the blank after inkjet printing a common ink pattern;
[0012] Positioning and applying the colored flashing dry particles on the surface of the blank after the inkjet printing of the glue pattern;
[0013] Apply transparent dry granule glaze on the surface of the body after applying colored flash dry granules;
[0014] The green body with the transparent dry granular glaze applied thereon is fired and polished to obtain the colorful glaring ceramic tile.
[0015] Preferably, the chemical composition of the glaze includes, by mass percentage, SiO2: 60~68%; Al2O3: 17~22%; Fe2O3: 0.1~0.3%; TiO2: 0.05~0.2%; CaO: 0.1~0.4%; MgO: 0.5~1.8%; K2O: 3.0~4.0%; Na2O: 2.5~3.5%; ZrO2: 5.0~8.5%; loss on ignition: 1~2%.
[0016] Preferably, the mineral composition of the glaze includes, by mass percentage, 28-35% potassium feldspar, 15-21% sodium feldspar, 12-18% kaolin, 12-18% quartz sand, 8-12% zirconium silicate, 1-5% alumina, 2-4% calcined talc, and 3-8% calcined kaolin.
[0017] Preferably, the glaze is applied by spraying or pouring; the specific gravity of the glaze is 1.4-1.5 g / cm 3 , glaze application amount is 450~650g / m 2 .
[0018] Preferably, the mineral composition of the transparent dry granule glaze includes, by mass percentage, 80-96% transparent dry granules and 4-20% transparent glaze; wherein, the chemical composition of the transparent dry granules includes, by mass percentage, SiO2: 58-64%; Al2O3: 10-14%; CaO: 9-11%; MgO: 1-2%; K2O: 4.5-6.5%; Na2O: 0.05-0.2%; ZnO: 5-7%; loss on ignition: 0.2-0.8%; wherein, the chemical composition of the transparent glaze includes, by mass percentage, SiO2: 40-50%; Al2O3: 9-13%; MgO: 4-7%; CaO: 4-9%; ZnO: 1.5-5%; BaO: 5.5-12%; K2O: 3.5-5.5%; Na2O: 1-2%; loss on ignition: 7-14%.
[0019] Preferably, the mineral composition of the transparent glaze includes, by mass percentage, 40-50% feldspar, 10-15% kaolin, 10-15% barium carbonate, 10-15% talc, 5-10% dolomite, 2-5% zinc oxide, and 5-10% limestone.
[0020] Preferably, the particle grading of the transparent dry particles includes: in mass percentage, 60-80 mesh: 8-12%, 80-100 mesh: 6-10%, 100-120 mesh: 8-15%, 120-140 mesh: 8-15%, 140-250 mesh: 50-60%, 250-325 mesh: 1-4%, and below 325 mesh: ≤2%.
[0021] Preferably, the transparent dry granular glaze is applied by pouring glaze; the specific gravity of the transparent dry granular glaze is 1.50-1.55 g / cm 3 , glaze application amount is 1100~1200 g / m 2 .
[0022] Preferably, the firing temperature is 1180-1220° C., and the firing period is 70-100 minutes.
[0023] In a third aspect, the present invention provides a colorful glare ceramic tile. The colorful glare ceramic tile is obtained according to the preparation method.
[0024] Beneficial Effects
[0025] The present invention is the first to apply the combination of unfired colored dry particles and zircon sand dry particles to prepare colorful glare ceramic tiles, broadening the application scope of zircon sand dry particles and achieving multiple visual effects of color and glitter. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a brick surface effect diagram of Example 1 of the present invention;
[0027] Figure 2 This is a brick surface effect diagram of comparative example 1 of the present invention;
[0028] Figure 3 This is a brick surface effect diagram of Comparative Example 3 of the present invention;
[0029] Figure 4 It is a brick surface effect diagram of comparative example 4 of the present invention. DETAILED DESCRIPTION
[0030] The present invention is further described by the following embodiments, and it should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention. The following is an exemplary description of the colored flashing dry particles, the colored glare ceramic tiles and the preparation method thereof according to the present invention.
[0031] The green body powder is pressed and formed to obtain a green body. The green body powder commonly used in the art can be used. For example, but not limited to, the chemical composition of the green body powder includes: in mass percentage, SiO2: 60-70%, Al2O3: 19-25%, Fe2O3: 0.5-1.5%, TiO2: 0.2-0.5%, CaO: 0.2-0.8%, MgO: 0.3-0.8%, K2O: 2.0-4.0%, Na2O: 1.5-3.5%, and loss on ignition: 4.0-6.0%.
[0032] The pressing machine can be used for pressing. The molding method includes but is not limited to dry pressing.
[0033] The green body is dried. The moisture content of the green body after drying can be controlled within 0.2-0.5wt%. The drying temperature can be 110-130°C. The drying time can be 0.5-1.5 hours.
[0034] Apply glaze on the surface of the blank. The function of the glaze is to cover the base color and defects of the blank and promote the color development of the inkjet pattern.
[0035] In some embodiments, the chemical composition of the glaze includes, by mass percentage, SiO2: 60~68%; Al2O3: 17~22%; Fe2O3: 0.1~0.3%; TiO2: 0.05~0.2%; CaO: 0.1~0.4%; MgO: 0.5~1.8%; K2O: 3.0~4.0%; Na2O: 2.5~3.5%; ZrO2: 5.0~8.5%; loss on ignition: 1~2%.
[0036] As an example, the mineral composition of the glaze includes, by mass percentage, 28-35% potassium feldspar, 15-21% sodium feldspar, 12-18% kaolin, 12-18% quartz sand, 8-12% zirconium silicate, 1-5% aluminum oxide, 2-4% calcined talc, and 3-8% calcined kaolin.
[0037] Prepare glaze slurry. The raw materials of the glaze slurry include glaze mineral composition, additives and water. In some embodiments of the glaze slurry, the mass ratio of the glaze mineral composition to water is 50~80:20~50. The additives of the glaze slurry include sodium tripolyphosphate and sodium carboxymethylcellulose. For example, sodium tripolyphosphate accounts for 0.1~0.5% of the total mass of the glaze mineral composition and water. For example, sodium carboxymethylcellulose accounts for 0.1~0.5% of the total mass of the glaze mineral composition and water. Weigh each raw material according to the raw material composition of the glaze slurry, and ball mill evenly until the glaze slurry passes through a 325 mesh sieve and the residue is ≤0.8wt%. When in use, water can be added to the above-mentioned glaze slurry to adjust the final desired glaze specific gravity.
[0038] The glaze is applied by spraying or pouring. Preferably, the glaze is applied by spraying. In some embodiments, the specific gravity of the glaze is 1.4-1.5 g / cm 3 , glaze application amount is 450~650 g / m 2 .
[0039] The surface of the green body after the glaze is applied is printed with a common ink pattern. The texture and color of the common ink pattern printed with the inkjet can be adaptively changed according to the needs. The ink pattern can be formed by printing the common ink with an inkjet machine.
[0040] After the ordinary ink pattern is printed on the surface of the blank, a glue pattern is printed on the surface of the blank. The glue pattern is printed by an inkjet printer. The glue pattern can be printed by a dual-channel inkjet printer. The grayscale of the glue pattern of each channel can be 40-60% and 40-60% respectively. Preferably, the amount of glue applied is less than 110 g / m 2 .
[0041] Prepare colored flashing dry particles. The raw material composition of the colored flashing dry particles includes: by mass percentage, 20-50% of unburned colored dry particles and 50-80% of zircon sand dry particles. If the proportion of zircon sand dry particles is too low, the flashing effect of the colored flashing dry particles is weak and the expected flashing effect cannot be achieved.
[0042] The mineral composition of the unburned colored dry granules includes basic minerals and colorants. The raw material composition of the basic minerals of the unburned colored dry granules includes: in terms of mass percentage, 5-40% potassium feldspar, 25-55% sodium feldspar, 20-45% kaolin, and 5-10% quartz powder.
[0043] In some embodiments, the chemical composition of the basic mineral of the unburned colored dry particles includes, by mass percentage, SiO2: 60~70%; Al2O3: 18~26%; Fe2O3: 0.1~0.3%; TiO2: 0.1~0.2%; MgO: 0.1~0.3%; CaO: 0.1~0.4%; K2O: 1~5%; Na2O: 4~6%; loss on ignition: 2~5%.
[0044] Prepare unfired colored dry particles. Weigh each raw material according to the basic mineral composition of the unfired colored dry particles, add water and additives, mix evenly, and prepare a basic glaze slurry of unfired colored dry particles; then add colorants to the basic glaze slurry of unfired colored dry particles, mix evenly again, and prepare a glaze slurry of unfired colored dry particles; spray dry the unfired colored dry particles glaze slurry to obtain unfired colored dry particles. The additives include but are not limited to sodium tripolyphosphate and sodium carboxymethyl cellulose. The colorant includes but is not limited to a wrapped red material. In some embodiments, the proportion of the colorant to the total mass of the unfired dry particles basic glaze slurry and the colorant is 5 to 15% (e.g., 10%).
[0045] In some embodiments of the unfired colored dry granule basic glaze slurry, the mass ratio of the basic mineral composition of the unfired colored dry granules to water is 60-70:30-40. The additives of the unfired colored dry granule basic glaze slurry include sodium tripolyphosphate and sodium carboxymethyl cellulose. For example, sodium tripolyphosphate accounts for 0.2-0.25% of the total mass of the basic mineral composition of the unfired colored dry granules and water. For example, sodium carboxymethyl cellulose accounts for 0.15-0.25% of the total mass of the basic mineral composition of the unfired colored dry granules and water. According to the raw material composition of the unfired colored dry granule basic glaze slurry, each raw material is weighed and ball-milled evenly until the glaze slurry passes through a 325-mesh sieve and the residue is ≤0.8wt%, thereby obtaining the unfired dry granule basic glaze slurry. Then, colorant is added to the unfired dry granule basic glaze slurry, and mixing is continued to be uniform to obtain the unfired colored dry granule glaze slurry. The unfired colored dry granule glaze slurry is sent to a spray drying tower for granulation. The glaze slurry is atomized by controlling the pressure of the spray gun, and a large amount of water evaporates at high temperature to obtain spherical dry granules. The particle size of the dry granules can be controlled by adjusting the spray gun pressure. The greater the spray gun pressure, the smaller the particle size of the dry granules. The moisture content of the dry granules can be controlled by adjusting the temperature of the spray tower. The lower the moisture content of the dry granules, the higher the strength. As an example, the moisture content of the unburned colored dry granules is controlled below 3wt%. Otherwise, the dry granules are easy to break, which is not conducive to reuse.
[0046] Zircon sand dry particles commonly used in the art may be used, for example, by purchasing zircon sand dry particles through commercial channels.
[0047] The particle size of the zircon sand dry particles can be 60-100 meshes. The finer the particle size of the zircon sand dry particles, the worse the flash effect. However, if the particle size of the zircon sand dry particles is too coarse, it is easy to contact with the polishing abrasive block and affect the flash effect.
[0048] Preferably, the particle size of the unburned colored dry particles is the same as that of the zircon sand dry particles. For example, the particle size of the unburned colored dry particles is 60-100 meshes. This allows the unburned colored dry particles and zircon sand dry particles to be better mixed and evenly mixed.
[0049] Colored glitter dry particles are applied on the surface of the blank after the glue pattern is printed by inkjet. The colored glitter dry particles can be applied by a dry particle distributing machine. The colored glitter dry particles are applied by the digital glue positioning process.
[0050] After the colored flash dry particles are applied, a fan is used to remove the dry particles that are not adhered and recycle them. The application amount of the colored flash dry particles can be 100-200g / m 2 If the amount of colored flash dry particles applied is too small, the flash effect will be poor. If the amount of colored flash dry particles applied is too large, some zircon sand dry particles will appear above the transparent dry particle glaze layer and are easily thrown away, affecting the flash effect.
[0051] The background technology mentioned that zircon sand dry particles are non-transparent and have their own opacity. When the prior art sets the zircon sand dry particles on the upper layer of the inkjet pattern layer, they are usually distributed in the corresponding position of the white pattern of the inkjet pattern layer to avoid a large area of zircon sand dry particle layer affecting the color of the inkjet pattern and deteriorating the coordination between the ceramic product and the layout design. The present invention creatively uses a combination of unfired colored dry particles and zircon sand dry particles to prepare colorful glare ceramic tiles, which has the following advantages: 1. The colored flashing dry particles containing zircon sand dry particles can be distributed at any position of the blank, which greatly broadens the scope of use of zircon sand dry particles. 2. The colored frit dry particles prepared by conventional methods have a low firing temperature. When used in combination with zircon sand dry particles, it will affect the exhaust of the blank, resulting in more bubbles in the transparent dry particle glaze layer, affecting the decorative effect and anti-fouling performance. The unfired colored dry particles of the present invention do not need to be fired at high temperature (high temperature melting), and the colorant has better color development. At the same time, the firing temperature is relatively high, which basically does not affect the exhaust performance of the body. The finally obtained colored glare ceramic tiles have high glaze quality and good anti-fouling performance.
[0052] After the colored flashing dry particles are applied, a transparent dry particle glaze is applied on the surface of the blank, and the conventional transparent dry particle glaze in the art can be used.
[0053] For example, the mineral composition of the transparent dry granule glaze includes: by mass percentage, transparent dry granules 80-96% and transparent glaze 4-20%. Transparent dry granules commonly used in the art can be used. For example, the chemical composition of the transparent dry granules may include: by mass percentage, SiO2: 58-64%; Al2O3: 10-14%; CaO: 9-11%; MgO: 1-2%; K2O: 4.5-6.5%; Na2O: 0.05-0.2%; ZnO: 5-7%; loss on ignition: 0.2-0.8%.
[0054] The particle gradation of the transparent dry particles may include: by mass percentage, 60-80 mesh: 8-12%, 80-100 mesh: 6-10%, 100-120 mesh: 8-15%, 120-140 mesh: 8-15%, 140-250 mesh: 50-60%, 250-325 mesh: 1-4%, below 325 mesh: ≤2%. Below 325 mesh refers to the part that passes through the 325 mesh screen. Controlling the particle gradation of the transparent dry particles within the above range can make the transparent dry particle glaze have fewer pores and better transparency after firing.
[0055] The transparent glaze commonly used in the art can be used. For example, the chemical composition of the transparent glaze may include, by mass percentage, SiO2: 40-50%; Al2O3: 9-13%; MgO: 4-7%; CaO: 4-9%; ZnO: 1.5-5%; BaO: 5.5-12%; K2O: 3.5-5.5%; Na2O: 1-2%; and loss on ignition: 7-14%.
[0056] As an example, the raw material composition of the transparent glaze includes: in terms of mass percentage, 40-50% feldspar, 10-15% kaolin, 10-15% barium carbonate, 10-15% talc, 5-10% dolomite, 2-5% zinc oxide, and 5-10% limestone. Feldspar includes but is not limited to potassium feldspar and / or sodium feldspar.
[0057] In some embodiments, the raw material composition of the transparent dry granular glaze slurry includes: by mass percentage, transparent dry granules 51-58%, transparent glaze 3-6%, glue 30-38%, and water 5-10%. According to the raw material composition of the transparent dry granular glaze slurry, each raw material is weighed and mixed evenly to obtain the transparent dry granular glaze slurry. During the use of the transparent dry granular glaze, water can be added to obtain the final desired specific gravity of the transparent dry granular glaze.
[0058] The transparent dry granular glaze can be glazed by pouring glaze. The specific gravity of the transparent dry granular glaze is 1.50-1.55 g / cm 3 , glaze application amount is 1100~1200 g / m 2 .
[0059] The green body with the transparent dry granular glaze is fired. It can be fired in a kiln. The firing temperature can be 1180~1220℃, and the firing cycle can be 70~100 minutes.
[0060] The fired green body is polished to obtain colorful glare ceramic tiles.
[0061] The colored glare ceramic tiles can also be edged, graded, waxed, packaged and stored as needed.
[0062] The present invention applies unfired colored dry particles to the preparation of colorful glare ceramic tiles for the first time. By using colored glittering dry particles composed of unfired colored dry particles and zircon sand dry particles, the influence of the opacity of the zircon sand dry particles themselves on the ink pattern decoration is avoided, the application scope of zircon sand is broadened, and multiple visual effects of color and glitter are achieved.
[0063] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0064] Example 1
[0065] A method for preparing a colored glare ceramic tile comprises the following steps:
[0066] Step 1. Apply glaze on the surface of the dried body. The mineral composition of the glaze includes: by mass percentage, potassium feldspar 31%, sodium feldspar 20%, kaolin 15%, quartz sand 15%, zirconium silicate 10%, aluminum oxide 2%, calcined talc 3%, calcined kaolin 4%. The chemical composition of the glaze includes: by mass percentage, SiO2: 65.63%, Al2O3: 18.00%, Fe2O3: 0.15%, TiO2: 0.14%, CaO: 0.27%, MgO: 1.09%, K2O: 3.51%, Na2O: 3.04%, ZrO2: 6.37%, loss on ignition: 1.80%. The glaze is applied by spraying. The specific gravity of the glaze is 1.45g / cm 3 , glaze application amount is 500g / m 2 .
[0067] Step 2. Inkjet print a normal ink pattern on the surface of the glazed body.
[0068] Step 3. After the ordinary ink pattern is printed, a glue pattern is printed on the surface of the blank by inkjet. The glue pattern is printed by inkjet printing in two channels. The grayscale of the glue pattern in each channel is 45% and 45% respectively.
[0069] Step 4. Apply colored flash dry particles on the surface of the blank after the inkjet printing of the glue pattern. The raw material composition of the colored flash dry particles includes: 20% of unburned colored dry particles and 80% of zircon sand dry particles by mass percentage. The mineral composition of the unburned colored dry particles includes basic minerals and red wrapped materials. The raw material composition of the basic minerals of the unburned colored dry particles includes: 20% potassium feldspar, 35% sodium feldspar, 35% kaolin, and 10% quartz powder by mass percentage. The chemical composition of the basic minerals of the unburned colored dry particles includes: SiO2: 66.81%; Al2O3: 21.65%; Fe2O3: 0.15%; TiO2: 0.13%; MgO: 0.2%; CaO: 0.25%; K2O: 2.94%; Na2O: 4.13%; ignition loss: 3.74%. The application amount of the colored flash dry particles is 110g / m 2 .
[0070] Step 5. Apply transparent dry granule glaze on the surface of the blank after applying the colored flash dry granules. The raw material composition of the transparent dry granule glaze slurry includes: by mass percentage, transparent dry granules 52%, transparent glaze 6%, glue 34%, and water 8%. The chemical composition of the transparent dry granules includes: by mass percentage, SiO2: 62.2%; Al2O3: 13%; CaO: 10.5%; MgO: 1%; K2O: 6.5%; Na2O: 0.1%; ZnO: 6.5%; loss on ignition: 0.2%. The particle grading of the transparent dry granules includes: by mass percentage, 60~80 mesh: 12%, 80~100 mesh: 8%, 100~120 mesh: 15%, 120~140 mesh: 8%, 140~250 mesh: 55%, 250~325 mesh: 1%, and below 325 mesh: 1%. The chemical composition of the transparent glaze includes: by mass percentage, SiO2: 47%; Al2O3: 12%; MgO: 6%; CaO: 8%; ZnO: 3%; BaO: 8%; K2O: 4.5%; Na2O: 1.5%; loss on ignition: 10%. The transparent dry granular glaze is glazed by pouring glaze. The specific gravity of the transparent dry granular glaze is 1.50g / cm 3 , glaze application amount is 1200 g / m 2 .
[0071] Step 7. Firing the green body after applying the transparent dry granular glaze. The firing temperature is 1200℃ and the firing cycle is 80 minutes.
[0072] Step 8. Polishing, edging, grading, and waxing.
[0073] Figure 1This is the brick surface effect diagram of Example 1. It can be seen that by using colored flashing dry particles composed of unfired colored dry particles and zircon sand dry particles, the influence of the opacity of zircon sand dry particles on the ink pattern decoration is avoided, the application scope of zircon sand is broadened, and multiple visual effects of color and flash are achieved.
[0074] Comparative Example 1
[0075] It is basically the same as Example 1: the only difference is that conventional colored frit dry particles are used to replace the unfired colored dry particles. The mineral composition of the colored frit dry particles includes basic minerals and colorants. The chemical composition of the basic minerals of the colored frit dry particles includes: in mass percentage, Al2O3: 14%, SiO2: 53%, CaO: 5%, MgO: 2%, K2O: 4%, Na2O: 3.5%, BaO: 6%, SrO: 5.5%, ZnO: 7%. According to the formula of the colored frit dry particles, each raw material is weighed, mixed evenly, and melted at 1400°C for 1.5 hours to obtain glass liquid; then the glass liquid is quenched and crushed to obtain a frit base material; then the frit base material is mixed with the colorant and put into a melting furnace, and after secondary firing, it is dried and crushed to obtain colored frit dry particles.
[0076] Figure 2 This is a brick surface effect diagram of comparative example 1. Comparative example 1 uses a combination of colored frit dry particles and zircon sand dry particles. Since the colored frit dry particles are fired at a low temperature, the exhaust of the green body is affected, resulting in more bubbles in the transparent dry particle glaze layer. After polishing, the bubbles are polished through, and the ultra-clean and bright nano-liquid used for waxing fills the pores in the form of white dots, affecting the decorative effect and anti-fouling performance.
[0077] Comparative Example 2
[0078] The method is basically the same as Example 1, except that the raw material composition of the base minerals of the unburned colored dry particles includes, by mass percentage, 20% potassium feldspar, 35% sodium feldspar, 25% kaolin, 10% quartz powder, and 10% wollastonite.
[0079] In this comparative example, since the unfired colored dry particles are at a relatively low temperature, more pores are formed by the dry particle polishing, and more white spots appear on the brick surface after waxing.
[0080] Comparative Example 3
[0081] It is basically the same as Example 1, except that the raw material composition of the colored flashing dry particles includes: 70% of unburned colored dry particles and 30% of zircon sand dry particles, by mass percentage.
[0082] Figure 3 This is the brick surface effect picture of Example 3. It can be seen that there are more unfired colored dry particles and fewer zircon sand dry particles, and the brick surface basically has no glitter effect.
[0083] Comparative Example 4
[0084] It is basically the same as Example 1: the only difference is that the raw material composition of the colored flashing dry particles includes: by mass percentage, 5% of unburned colored dry particles and 95% of zircon sand dry particles.
[0085] Figure 4 This is the brick surface effect picture of comparative example 4. It can be seen that there are fewer unfired colored dry particles and more zircon sand dry particles. Due to the poor transparency of zircon sand, the brick surface effect does not match the pattern layout design.
Claims
1. A colored flashing dry granule, characterized in that: The raw material composition of the colored flashing dry particles includes: in percentage by mass, 20-50% of unburned colored dry particles and 50-80% of zircon sand dry particles; the unburned colored dry particles include basic minerals and colorants; wherein the chemical composition of the basic minerals of the unburned colored dry particles is: in percentage by mass, SiO2: 60-70%; Al2O3: 18-26%; Fe2O3: 0.1-0.3%; TiO2: 0.1-0.2%; MgO: 0.1-0.3%; CaO: 0.1-0.4%; K2O: 1-5%; Na2O: 4-6%; loss on ignition: 2-5%; the raw material composition of the basic minerals of the unburned colored dry particles is: in percentage by mass, 5-40% of potassium feldspar, 25-55% of sodium feldspar, 20-45% of kaolin, and 5-10% of quartz powder.
2. The colored flashing dry particles according to claim 1, characterized in that: The particle size of the unburned colored dry particles is 60-100 meshes; the particle size of the zircon sand dry particles is 60-100 meshes.
3. The colored flashing dry particles according to claim 1, characterized in that: The preparation method of the unfired colored dry particles comprises: weighing various raw materials according to the raw material composition of the basic minerals of the unfired colored dry particles, adding water and an auxiliary agent, and mixing them evenly to prepare a basic glaze slurry of the unfired colored dry particles; then adding a colorant to the basic glaze slurry of the unfired colored dry particles, mixing them evenly again, and preparing a glaze slurry of the unfired colored dry particles; spray drying and granulating the unfired colored dry particles glaze slurry to obtain the unfired colored dry particles.
4. A method for preparing a colored glare ceramic tile, characterized in that: The preparation method comprises the following steps: Applying glaze on the surface of the body; Inkjet printing a common ink pattern on the surface of the body after the glaze is applied; Inkjet printing a glue pattern on the surface of the blank after inkjet printing a common ink pattern; Positioning and applying the colored glitter dry particles according to any one of claims 1 to 3 on the surface of the blank after the inkjet printing of the glue pattern; Apply transparent dry granule glaze on the surface of the body after applying colored flash dry granules; The green body with the transparent dry granular glaze applied thereon is fired and polished to obtain the colorful glaring ceramic tile.
5. The preparation method according to claim 4, characterized in that: The chemical composition of the glaze includes, by mass percentage, SiO2: 60~68%; Al2O3: 17~22%; Fe2O3: 0.1~0.3%; TiO2: 0.05~0.2%; CaO: 0.1~0.4%; MgO: 0.5~1.8%; K2O: 3.0~4.0%; Na2O: 2.5~3.5%; ZrO2: 5.0~8.5%; loss on ignition: 1~2%.
6. The preparation method according to claim 4, characterized in that: The glaze is applied by spraying or pouring; the specific gravity of the glaze is 1.4-1.5g / cm 3 , glaze application amount is 450~650g / m 2 .
7. The preparation method according to claim 4, characterized in that: The mineral composition of the transparent dry granule glaze includes, by mass percentage, 80-96% of transparent dry granules and 4-20% of transparent glaze; wherein, the chemical composition of the transparent dry granules includes, by mass percentage, SiO2: 58-64%; Al2O3: 10-14%; CaO: 9-11%; MgO: 1-2%; K2O: 4.5-6.5%; Na2O: 0.05-0.2%; ZnO: 5-7%; loss on ignition: 0.2-0.8%; wherein, the chemical composition of the transparent glaze includes, by mass percentage, SiO2: 40-50%; Al2O3: 9-13%; MgO: 4-7%; CaO: 4-9%; ZnO: 1.5-5%; BaO: 5.5-12%; K2O: 3.5-5.5%; Na2O: 1-2%; loss on ignition: 7-14%.
8. The preparation method according to claim 7, characterized in that: The mineral composition of the transparent glaze includes, by mass percentage, 40-50% feldspar, 10-15% kaolin, 10-15% barium carbonate, 10-15% talc, 5-10% dolomite, 2-5% zinc oxide, and 5-10% limestone.
9. The preparation method according to claim 7, characterized in that: The particle grading of the transparent dry particles includes: in mass percentage, 60-80 mesh: 8-12%, 80-100 mesh: 6-10%, 100-120 mesh: 8-15%, 120-140 mesh: 8-15%, 140-250 mesh: 50-60%, 250-325 mesh: 1-4%, and below 325 mesh: ≤2%.
10. The preparation method according to claim 4, characterized in that The transparent dry granular glaze is applied by pouring glaze; the specific gravity of the transparent dry granular glaze is 1.50-1.55 g / cm 3 , glaze application amount is 1100~1200 g / m 2 .
11. A colorful glare ceramic tile, characterized in that: The colorful glare ceramic tile is obtained according to the preparation method described in any one of claims 4 to 10.