An intelligent preparation method for water-resistant silicon carbide ceramic-based composite materials
By using the mixed ball milling and deposition technology of yttrium oxide powder, silicon carbide powder and polyvinyl alcohol in SiC ceramic matrix composite materials, combined with the analysis of the temperature diagram of the infiltration working conditions, the reaction infiltration time is controlled, and the SiC ceramic matrix problem is solved. The degradation problem of composite materials in the aero-engine environment improves the mechanical properties and density of the materials.
Patent Information
- Application Number
- CN202411019741.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing SiC ceramic matrix composite materials react with water vapor and oxygen in the aero-engine gas environment, resulting in degradation, and the existing EBCs barrier coating has the risk of cracking, affecting the safety performance of the aero-engine, and the preparation by the reactive infiltration method needs to be strictly controlled The reaction infiltration time should be adjusted to avoid problems of excessive temperature or insufficient reaction.
Yttrium oxide powder, silicon carbide powder, polyvinyl alcohol and solvent are mixed and ball milled, boron nitride and silicon carbide are deposited to form a silicon carbide fiber preform, and water and oxygen resistant silicon carbide ceramic matrix composites are prepared through impregnation and pyrolysis. Analyze the temperature chart of the infiltration working conditions, predict the adequacy of the exothermic reaction, and regulate the reaction infiltration time to ensure sufficient reaction between silicon and carbon.
It improves the mechanical properties and density of water-oxygen-resistant silicon carbide ceramic matrix composite materials, reduces the risk of interface damage by high temperatures, and ensures high densification and safety performance of the material.
Smart Images

Figure CN118546003B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of preparation of silicon carbide ceramic-based composite materials, and in particular to an intelligent preparation method of water-oxidation resistant silicon carbide ceramic-based composite materials. Background Art
[0002] Silicon carbide (SiC) ceramic matrix composite is a high-performance composite material. It not only has the characteristics of high specific strength, high temperature resistance, corrosion resistance, and low density of SiC ceramics, but also has the advantages of SiC fiber reinforcement and toughening. It has broad application prospects and market value in aerospace, automotive brake systems and other fields. With the continuous development of the aviation industry, the performance of the new generation of aircraft has been significantly improved, which has posed higher challenges to the performance of aircraft generators. In the fuel gas environment of aircraft engines, the SiC ceramic matrix will react with water vapor and oxygen to generate volatile substances, causing the SiC ceramic matrix composite to degrade. At present, the method of applying EBCs (environmental barrier coatings) on the surface of SiC ceramic matrix composites is usually adopted, but there is still a risk of cracking after long-term use, which greatly affects the safety performance of aircraft engines. There is an urgent need for a water- and oxygen-resistant silicon carbide ceramic matrix composite material.
[0003] The preparation of water-oxidation-resistant silicon carbide ceramic-based composites by reactive melt infiltration (RMI) is relatively simple and low in cost. The thermal conductivity of water-oxidation-resistant silicon carbide ceramic-based composites is high, but the reaction infiltration time needs to be strictly controlled. Since the reaction of silicon (Si) and carbon (C) is an exothermic reaction, if the reaction infiltration time is too long, the local temperature may be too high, and the interface of the water-oxidation-resistant silicon carbide ceramic-based composite material may be easily damaged, which in turn causes a large amount of thermal damage to the fiber, greatly affecting the mechanical properties of the water-oxidation-resistant silicon carbide ceramic-based composite material; if the reaction infiltration time is too short, the Si melt may fail to fully fill the pores inside the preform, and the reaction between Si and carbon is insufficient, resulting in a low degree of matrix densification of the water-oxidation-resistant silicon carbide ceramic-based composite material. Summary of the invention
[0004] In order to solve the above technical problems, the present application provides an intelligent preparation method of water-oxidation resistant silicon carbide ceramic-based composite materials to solve the existing problems.
[0005] The intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material of the present application adopts the following technical scheme:
[0006] An embodiment of the present application provides an intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material, the method comprising the following steps:
[0007] Mixing and ball-milling yttrium oxide powder, silicon carbide powder, polyvinyl alcohol and solvent according to a preset mass ratio to obtain a mixed slurry;
[0008] The silicon carbide fibers are braided and cut to obtain a first silicon carbide fiber preform, and boron nitride and silicon carbide are deposited to obtain a second silicon carbide fiber preform;
[0009] The second silicon carbide fiber preform is impregnated in the mixed slurry to obtain an impregnated preform; the impregnated preform is cut, laminated, dried, cured, and pyrolyzed in sequence to obtain a fiber preform;
[0010] The fiber preform is impregnated in a phenolic resin, and then subjected to secondary pyrolysis and reactive infiltration to obtain a water- and oxygen-resistant silicon carbide ceramic-based composite material. During the reactive infiltration process, the control process of the reactive infiltration time is specifically as follows:
[0011] A1, obtain the infiltration working temperature diagram at each acquisition moment;
[0012] A2, based on the temperature diffusion decrease of any pixel in the local temperature neighborhood and the increase of the neighborhood temperature, obtain the exothermic reaction pixel suspicion of any pixel;
[0013] A3, based on the difference in the suspected degrees of all exothermic reaction pixels in the infiltration condition temperature map within a preset acquisition period between pixels, the infiltration reaction area in the infiltration condition temperature map is screened out;
[0014] A4, based on the number of pixels corresponding to the exothermic reaction pixel suspicion degree that meets the threshold condition in each infiltration reaction area and the increase in the neighborhood temperature of all pixels in each infiltration reaction area, determine the degree of exothermic reaction sufficiency of each infiltration reaction area;
[0015] A5, based on the degree of exothermic reaction of each infiltration reaction area at all sampling moments, predict the predicted value of the degree of exothermic reaction at the next sampling moment; combine the prediction results of all infiltration reaction areas at the next sampling moment for several consecutive times to adjust the reaction infiltration time.
[0016] Preferably, the yttrium oxide powder, silicon carbide powder, polyvinyl alcohol and solvent in the mixed ball mill are mixed according to a mass ratio of (20-40):(1-10):(7-15):(35-50).
[0017] Preferably, the solvent is one or a combination of ethanol, isopropanol or xylene.
[0018] Preferably, obtaining the second silicon carbide fiber preform further comprises: depositing boron carbide on the first silicon carbide fiber preform to obtain a BN interface layer; and depositing silicon carbide on the basis of the BN interface layer to obtain the second silicon carbide fiber preform.
[0019] Preferably, the specific deposition parameters of the BN interface layer when boron nitride is used for deposition are: boron trichloride is used as the boron source, ammonia is used as the nitrogen source, hydrogen is used as the dilution gas, the deposition temperature is set to 700ºC, and the deposition pressure is set to 5kPa; the specific deposition parameters of the second silicon carbide fiber preform when silicon carbide is used for deposition are: trichloromethylsilane is used as the gaseous precursor, hydrogen is used as the carrier gas, argon is used as the dilution gas, the deposition temperature is 1100°C, and the deposition pressure is 5kPa.
[0020] Preferably, the process of obtaining the impregnated preform is to perform pressure impregnation and vacuum impregnation in the mixed slurry in sequence.
[0021] Preferably, the method for determining the exothermic reaction pixel suspicion degree comprises:
[0022] For each pixel in the local temperature neighborhood with any pixel as the central pixel, count the step length from each pixel to the central pixel, and take the pixels with the same step length as the same circle pixels; arrange them from small to large in order, and form the same circle pixels with the same step length into each circle pixel;
[0023] Calculate the difference in the temperature mean between adjacent circle pixels, and take the cumulative sum of the differences between all adjacent circle pixels in the local temperature neighborhood of the central pixel as the temperature diffusion decrease of the central pixel in the local temperature neighborhood; wherein the difference is the difference between the temperature mean of the circle with a small step size and the circle with a large step size in the adjacent circle pixels;
[0024] The difference between the temperature mean of the pixels in the local temperature neighborhood of the central pixel and the temperature mean of the pixels in the infiltration working condition temperature map to which it belongs is taken as the increase of the neighborhood temperature of the central pixel in the local temperature neighborhood;
[0025] The product of the temperature diffusion decrease and the neighborhood temperature increase is taken as the exothermic reaction pixel suspicion of the central pixel.
[0026] Preferably, the screening process of the infiltration reaction area includes:
[0027] Calculate the cumulative sum of the exothermic reaction pixel suspicion of any pixel in the infiltration working condition temperature map within the preset acquisition period as the exothermic reaction credibility of any pixel;
[0028] The exothermic reaction credibility of each pixel is used to replace the temperature value of the corresponding pixel in the infiltration working condition temperature map, and the result after replacement is used as the exothermic reaction credibility map; the exothermic reaction credibility map is segmented into superpixels to obtain a number of superpixel blocks;
[0029] Calculate the exothermic reaction credibility mean of all pixels in each superpixel block; perform threshold segmentation on the exothermic reaction credibility mean of all superpixel blocks, output the credible threshold, and correspond the superpixel blocks whose exothermic reaction credibility mean is greater than or equal to the credible threshold to the area in the infiltration industrial control temperature map, which is recorded as the infiltration reaction area.
[0030] Preferably, the method for determining the degree of sufficiency of the exothermic reaction comprises:
[0031] The exothermic reaction pixel suspicion of all pixels in the infiltration working condition temperature map at any acquisition time is segmented by threshold, and the suspicion threshold is output, and the pixels whose exothermic reaction pixel suspicion is greater than or equal to the suspicion threshold are regarded as exothermic reaction pixels; the number of exothermic reaction pixels in any infiltration reaction area is counted;
[0032] Calculate the average value of the neighborhood temperature increase of all pixels in any infiltration reaction area at any acquisition moment;
[0033] The number of exothermic reaction pixels and the average value of the neighborhood temperature increase are combined to obtain the degree of sufficiency of the exothermic reaction.
[0034] Preferably, the exothermic reaction sufficiency of each infiltration reaction area at all sampling moments is used to predict the predicted value of the exothermic reaction sufficiency at the next sampling moment; and the reaction infiltration time is regulated by combining the prediction results of all infiltration reaction areas at the next sampling moment for several consecutive times, specifically:
[0035] The exothermic reaction sufficiency of any infiltration reaction region at all sampling moments is used to form an exothermic reaction sufficiency sequence of the corresponding infiltration reaction region;
[0036] Predicting the predicted value of the exothermic reaction sufficiency of the exothermic reaction sufficiency sequence of each infiltration reaction area at the next acquisition moment;
[0037] The normalized value of the cumulative sum of the predicted values of the exothermic reaction sufficiency of all infiltration reaction areas at the next acquisition moment is used as the predicted exothermic reaction degree of the current reactive infiltration process;
[0038] When the predicted exothermic reaction degree of the reactive infiltration process is lower than the preset predicted reaction threshold value for a preset number of consecutive times, the heating of the reactive infiltration process is stopped.
[0039] The beneficial effects of this application are:
[0040] The present application solves the problem that when there are multiple suspected pixels with high temperature values that diffuse to the surrounding temperatures in the local temperature neighborhood and the temperature diffusion decline of the pixels at each acquisition moment, the temperature diffusion decline cannot accurately reflect the reaction temperature characteristics of the system, thereby improving the accuracy of subsequent silicon carbide reaction pixel identification and facilitating the regulation of the reaction infiltration time of the reaction infiltration process; the present application predicts the predicted value of the exothermic reaction sufficiency at the next acquisition moment based on the silicon carbide reaction sufficiency of any infiltration reaction area at each acquisition moment, thereby regulating the reaction infiltration time, and reducing the risk of the interface of the water-oxygen-resistant silicon carbide ceramic-based composite material being damaged by long-term high temperature while ensuring the sufficient reaction of silicon and carbon and the high density of the matrix of the water-oxygen-resistant silicon carbide ceramic-based composite material, thereby improving the mechanical properties of the water-oxygen-resistant silicon carbide ceramic-based composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0042] Figure 1 A flowchart of the steps of an intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material provided in one embodiment of the present application;
[0043] Figure 2 A schematic diagram of a process flow for preparing a water-oxidation-resistant silicon carbide ceramic-based composite material provided in one embodiment of the present application;
[0044] Figure 3 A schematic diagram of the structure of a second silicon carbide fiber preform provided in one embodiment of the present application;
[0045] Figure 4 A schematic diagram of a post-processing process of an impregnated preform provided in one embodiment of the present application;
[0046] Figure 5 A flow chart of a control process of reaction infiltration time provided in one embodiment of the present application;
[0047] Figure 6 A schematic diagram of temperature diffusion drop provided for one embodiment of the present application;
[0048] Figure 7 A schematic diagram of a bending stress-displacement curve of a water-oxidation-resistant silicon carbide ceramic-based composite material provided in one embodiment of the present application;
[0049] Figure 8A schematic diagram of a tensile stress-displacement curve of a water-oxidation-resistant silicon carbide ceramic-based composite material provided in one embodiment of the present application. DETAILED DESCRIPTION
[0050] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the following is a detailed description of the intelligent preparation method of a water-resistant silicon carbide ceramic-based composite material proposed in the present application, its specific implementation method, structure, characteristics and effects, in combination with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "another embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.
[0051] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs.
[0052] The specific scheme of the intelligent preparation method of the water-oxidation resistant silicon carbide ceramic-based composite material provided by the present application is described in detail below with reference to the accompanying drawings.
[0053] Embodiment 1:
[0054] An embodiment of the present application provides an intelligent preparation method for a water-resistant silicon carbide ceramic-based composite material. For the preparation flow chart, please refer to Figure 1 , the specific preparation process is as follows:
[0055] The preparation process of the water-resistant silicon carbide ceramic matrix composite material consists of the steps of mixed ball milling, preparation of the first silicon carbide fiber preform, deposition, slurry impregnation, post-treatment of the impregnated preform and preparation of the water-resistant silicon carbide ceramic matrix composite material. The schematic diagram of the preparation process of the water-resistant silicon carbide ceramic matrix composite material is shown in the attached figure. Figure 2 As shown, specifically:
[0056] Yttrium oxide powder, silicon carbide powder, polyvinyl alcohol and solvent are mixed and ball-milled according to a preset mass ratio to obtain a mixed slurry; a first silicon carbide fiber preform is obtained by weaving and cutting silicon carbide fibers, and a second silicon carbide fiber preform is obtained by depositing boron nitride and silicon carbide; the second silicon carbide fiber preform is impregnated in the mixed slurry to obtain an impregnated preform; the impregnated preform is sequentially cut, laminated, dried, cured and subjected to primary pyrolysis to obtain a fiber preform; the fiber preform is impregnated in a phenolic resin, and subjected to secondary pyrolysis and reactive infiltration to obtain a water-oxidation-resistant silicon carbide ceramic-based composite material.
[0057] Mixing ball mill:
[0058] Yttrium oxide (Y2O3) powder, silicon carbide powder, polyvinyl alcohol and solvent are mixed in a mass ratio of 20:1:7:40, wherein the particle size of SiC powder is 0.01-20μm, the particle size of Y2O3 powder can be 0.01-10μm, and the solvent is a combination of ethanol and isopropanol. The mixture is sent to a ball mill for ball milling to obtain a mixed slurry, wherein the diameter of the corundum balls in the ball mill is 10mm-20mm, the ball milling time is 24-48h, and the ball mill speed is 250-350r / min.
[0059] Preparation of the first preform of silicon carbide fiber:
[0060] Silicon carbide is woven into silicon carbide fiber cloth by a plain weave method, and then the silicon carbide fiber cloth is cut into appropriate sizes by a two-dimensional plain weave machine, and is layered on a graphite mold, and the graphite mold is fixed and clamped by graphite bolts on all sides to obtain a first silicon carbide fiber preform, wherein the thickness of the first silicon carbide fiber preform can be 0.1 to 1 mm.
[0061] Deposition:
[0062] The interface layer material of this process is boron nitride, and a BN interface layer of 0.1 to 5 μm is deposited on the first silicon carbide fiber preform by chemical vapor infiltration. The specific deposition parameters are: boron trichloride (BCl3) is used as the boron source, ammonia (NH3) is used as the nitrogen source, hydrogen (H2) is used as the dilution gas, the deposition temperature is set to 700ºC, and the deposition pressure is set to 5kPa. Furthermore, in order to avoid the damage to the BN interface layer during the subsequent pyrolysis process, a certain amount of SiC matrix is further deposited on the basis of the obtained BN interface layer by chemical vapor infiltration to obtain the second silicon carbide fiber preform. The specific deposition parameters are: trichloromethylsilane (CH3SiCl3) is used as the gaseous precursor, H2 is used as the carrier gas, argon (Ar) is used as the dilution gas, the deposition temperature is 1100°C, the deposition pressure is 5kPa, and the thickness of the SiC matrix can be determined by the implementer according to the actual situation. The schematic diagram of the structure of the second silicon carbide fiber preform is shown in the attached figure. Figure 3 As shown, 1 is SiC fiber, 2 is BN interface layer, and 3 is SiC matrix.
[0063] Slurry impregnation:
[0064] The second silicon carbide fiber preform is impregnated in a mixed slurry containing Y2O3, first by pressure impregnation, wherein the pressure impregnation time is 30 to 60 minutes, the pressure of the pressure impregnation is 0.8 MPa, and then by vacuum impregnation, wherein the vacuum impregnation time is 30 to 60 minutes, to obtain an impregnated preform.
[0065] Post-treatment of impregnated preforms:
[0066] The impregnated preform is cut, laminated, dried, cured, and pyrolyzed in sequence to obtain a fiber preform. The schematic diagram of the post-processing process of the impregnated preform is shown in the attached figure. Figure 4 As shown, the cutting and lamination parameters are confirmed by the implementer according to the specific situation, the drying temperature is 80-120°C, the drying time is 0.5-3h, the curing temperature is 80-300°C, the curing pressure is 0.1-20MPa, the curing time is 0.5-10 hours, and the primary pyrolysis temperature can be 500-1000°C, and the time is 0.5-5 hours.
[0067] Preparation of water-resistant silicon carbide ceramic matrix composites:
[0068] The fiber preform is impregnated in a phenolic resin, and undergoes secondary pyrolysis and reactive infiltration to obtain a water-oxidation-resistant silicon carbide ceramic-based composite material, wherein the secondary pyrolysis temperature can be 500-1000°C, the time can be 0.5-5 hours, the reactive infiltration temperature is 1280-1500°C, and the reactive infiltration time is 60-180 minutes.
[0069] Among them, if the reaction infiltration time is too long, it may cause the local temperature to be too high, and the interface of the water-resistant silicon carbide ceramic-based composite material is easily damaged, which in turn causes a large amount of thermal damage to the fiber, greatly affecting the mechanical properties of the water-resistant silicon carbide ceramic-based composite material; if the reaction infiltration time is too short, it may cause the Si melt to fail to fully fill the pores inside the preform, and the reaction between Si and carbon is insufficient, resulting in a low degree of matrix densification of the water-resistant silicon carbide ceramic-based composite material. Accordingly, based on the above problems, this application controls the reaction infiltration time. The control process flow chart of the reaction infiltration time is shown in the attached figure. Figure 5 As shown, specifically:
[0070] A1, obtain the infiltration working temperature diagram at each acquisition moment.
[0071] In this embodiment, the time point after 60 minutes of reactive infiltration is used as the acquisition starting point, and a high-temperature thermal imager is used to collect thermal imaging images of the reactive infiltration working conditions during the preparation process. The acquisition time interval in this embodiment is 30 seconds. The thermal imaging images obtained at each acquisition moment are respectively used as input, and the bilateral filtering algorithm is used for denoising and enhancement, and each output thermal imaging image is recorded as a temperature map of the infiltration working condition. Among them, the bilateral filtering algorithm is a well-known technology and will not be repeated.
[0072] At this point, the infiltration condition temperature diagram at each acquisition moment can be obtained.
[0073] A2, based on the temperature diffusion decrease of any pixel in the local temperature neighborhood and the increase of the neighborhood temperature, obtain the exothermic reaction pixel suspicion of any pixel.
[0074] In the process of reactive infiltration to generate SiC matrix, since the Si-C system reaction is an exothermic reaction, a large amount of heat is released locally, which promotes the melting of Si particles. The Si melt infiltrates into the pores of the porous preform under the action of capillary force, so that the infiltration and reaction proceed simultaneously, and the SiC matrix gradually forms a layered distribution on the outside of the fiber bundle.
[0075] This application takes the infiltration working condition temperature diagram at the t-th acquisition moment as an example, takes the i-th pixel as the center, and obtains a 9*9 window as the local temperature neighborhood of pixel i. Pure Si particles and Si melt are heated evenly, with small temperature differences, but are easily affected by the exothermic reaction of the Si-C system. The pixels where the Si-C system reaction occurs are recorded as exothermic reaction pixels. The method for determining whether a pixel is an exothermic reaction pixel is as follows: within the local temperature neighborhood of pixel i, the more the temperature value of the central pixel diffuses and decreases toward the boundary of the local temperature neighborhood, the more likely pixel i is an exothermic reaction pixel. The schematic diagram of temperature diffusion decrease is shown in the attached figure. Figure 6 As shown, in Figure 6 In the figure, the higher the temperature, the darker the color. At the same time, since the infiltration and reaction are carried out simultaneously, it is very likely that there will be multiple exothermic reaction pixels with high temperature values in a local temperature neighborhood.
[0076] This application obtains the exothermic reaction pixel suspicion of any pixel based on the temperature diffusion drop and the neighborhood temperature increase in the local temperature neighborhood of the pixel, which is used to reflect the possibility that the pixel belongs to the exothermic reaction pixel. In this application, the exothermic reaction pixel suspicion of the pixel is specifically calculated by multiplying the temperature diffusion drop and the neighborhood temperature increase.
[0077] In this embodiment, the step lengths from all pixels to the center pixel are counted, and pixels with the same step length are regarded as pixels in the same circle, and are arranged according to the step lengths. The pixels in the same circle with the smallest step length are regarded as the first circle of pixels, and so on, and a total of o circles of pixels are obtained. In this embodiment, the value of o is 5, and the implementer can set it according to the actual situation.
[0078] Based on the above analysis, the temperature diffusion decrease of the pixel in the local temperature neighborhood can be obtained: : ; is the temperature diffusion decrease of the pixel in the local temperature neighborhood, is the total number of circles in the local temperature neighborhood of each central pixel, , are the mean temperatures of all pixels in the uth circle and the u+1th circle in the local temperature neighborhood, is the number of adjacent circles in the local temperature neighborhood.
[0079] It should be understood that when the temperature value of a pixel farther from the central pixel in the local temperature neighborhood is lower, that is, The larger it is, the more the temperature from the central pixel to the boundary pixel in the local temperature neighborhood has a gradually decreasing characteristic, and the more it conforms to the characteristic of diffusion from high temperature values to low temperature values. The higher the temperature diffusion decreases, the more likely the pixel is an exothermic reaction pixel of the Si-C system reaction, and the greater the suspicion of the exothermic reaction pixel.
[0080] At the same time, if the temperature of the pixel in the local temperature neighborhood is larger than the temperature of the overall infiltration condition temperature map, it means that the temperature in the local temperature neighborhood of the pixel is higher, and it is more likely to be an exothermic reaction pixel. The specific judgment method is:
[0081] The difference between the temperature mean of all pixels in the local temperature neighborhood of the pixel and the temperature mean of all pixels in the infiltration condition temperature map at the acquisition time t is taken as the neighborhood temperature increase of the corresponding pixel in the local temperature neighborhood.
[0082] It should be understood that the greater the increase in neighborhood temperature, the higher the overall temperature in the local temperature neighborhood, the greater the temperature difference between the local temperature neighborhood temperature and the infiltration condition temperature diagram, the more likely it is that continuous exothermic reaction pixels will occur in the local temperature neighborhood, the more likely the pixel will be an exothermic reaction pixel of the Si-C system reaction, and the greater the suspicion of the exothermic reaction pixel.
[0083] A3, based on the difference in the suspicion of all exothermic reaction pixels in the infiltration condition temperature map within a preset acquisition period between pixels, the infiltration reaction area in the infiltration condition temperature map is screened out.
[0084] In the infiltration temperature diagram, there is an infiltration reaction area where Si-C system reaction can occur, which has significant temperature change characteristics and is composed of exothermic reaction pixels. In the infiltration temperature diagram, there is also a Si infiltrant area, which is responsible for providing melt to the infiltration reaction area and infiltrating the preform.
[0085] In order to avoid insufficient reaction of the Si-C system when the reaction infiltration time is short, not all pixels in the infiltration reaction area undergo Si-C system reaction within a single acquisition moment. Accordingly, the present application extracts the infiltration working temperature map within the preset acquisition period, calculates the cumulative sum of the exothermic reaction pixel suspicion of any pixel in the infiltration working temperature map within the preset acquisition period, and uses it as the exothermic reaction credibility of any pixel to reflect the credibility of the pixel having undergone Si-C system reaction within the preset acquisition period, wherein the preset acquisition period in this embodiment is M acquisition moments after the acquisition start point, and the value of M in this embodiment is 20.
[0086] Next, the exothermic reaction credibility of each pixel is used to replace the temperature value of the corresponding pixel in the infiltration working condition temperature map, and all pixels are traversed. The replaced result is used as the exothermic reaction credibility map, and the exothermic reaction credibility map is used as input, and the SLIC (Simple Linear Iterative Clustering) simple iterative linear segmentation algorithm is used to output all superpixel blocks. Among them, the SLIC algorithm is a well-known technology and will not be repeated here. In other embodiments of the present application, other superpixel block segmentation algorithms such as SEEDS (Superpixels Extracted via Energy-Driven Sampling) can also be used to perform superpixel segmentation on the exothermic reaction credibility map.
[0087] Calculate the exothermic reaction credibility mean of all pixels in each superpixel block; use the exothermic reaction credibility mean of all superpixel blocks as the input of the Otsu method, output the credible threshold, and record the area in the infiltration industrial control temperature map corresponding to the superpixel blocks whose exothermic reaction credibility mean is greater than or equal to the credible threshold as the infiltration reaction area. The Otsu method is a well-known technology and will not be described in detail. In other embodiments of the present application, the global threshold method and the like can also be used for threshold segmentation.
[0088] A4, based on the number of pixels corresponding to the exothermic reaction pixel suspicion degree that meet the threshold conditions in each infiltration reaction area and the increase in the neighborhood temperature of all pixels in each infiltration reaction area, the degree of exothermic reaction sufficiency of each infiltration reaction area is determined.
[0089] The key to generating SiC matrix by reactive infiltration lies in the penetration of Si melt into the preform. As the temperature of Si-C reaction element increases, the viscosity of liquid Si melt decreases, and the viscous resistance decreases, which helps to increase the penetration rate of the melt. That is, the molten liquid Si can more fully fill the voids in the preform, so that there are a large number of Si-C reaction elements in the infiltration reaction area, which can improve the density of the SiC matrix of the water-oxidation resistant silicon carbide ceramic-based composite material and avoid a large amount of free Si and free carbon remaining in the matrix when the reaction between liquid Si and carbon is insufficient, which seriously affects the high-temperature mechanical properties of the composite material.
[0090] This application takes the collection time r as an example, r needs to be greater than or equal to M, M is set by the implementer according to the actual situation, the first M collection times are used to divide the infiltration reaction area, and after the collection time M, it is judged whether the reaction is sufficient.
[0091] According to the number of exothermic reaction pixels and the increase in neighborhood temperature in any infiltration reaction area at the acquisition time r, the degree of exothermic reaction in the corresponding infiltration reaction area at the acquisition time r is obtained, which is used to reflect the degree of sufficiency of the Si-C system reaction in the infiltration reaction area at the acquisition time r.
[0092] Among them, in this embodiment, in the infiltration working condition temperature map at the acquisition time r, the exothermic reaction pixel suspicion of all pixels is used as the input of the Otsu method, the suspected threshold is output, and the pixels whose exothermic reaction pixel suspicion is greater than or equal to the suspected threshold are used as exothermic reaction pixels; and the number of exothermic reaction pixels in any infiltration reaction area is counted.
[0093] It should be understood that the greater the number of exothermic reaction pixels, the more pixels may have Si-C system reaction in the infiltration reaction area at the acquisition time r, and the more complete the Si-C system reaction in the infiltration reaction area, the greater the degree of completeness of the exothermic reaction.
[0094] In this embodiment, the average value of the increase in the neighborhood temperature of all pixels in any infiltration reaction area at the rth acquisition moment is calculated.
[0095] It should be understood that when the overall temperature of the infiltration reaction zone is higher, the viscosity of the liquid Si melt in the infiltration reaction zone may be lower, the melt permeability is higher, the molten liquid Si can more fully fill the gaps in the preform, the more Si-C system reactions can occur in the infiltration reaction zone, and the degree of exothermic reaction is greater.
[0096] The number of exothermic reaction pixels and the average value of the neighborhood temperature increase are combined to obtain the degree of exothermic reaction sufficiency of any infiltration reaction area at the acquisition time r.
[0097] It can be understood that fusion can be divided into forward fusion and reverse fusion. This embodiment adopts the forward fusion method. Forward fusion is a fusion method such as addition and multiplication between data. The specific forward fusion method is determined by the implementer according to the actual situation. The application does not impose any special restrictions.
[0098] In this embodiment, the product of the number of exothermic reaction pixels in any infiltration reaction area and the increase in the temperature of the neighboring area is used as the degree of exothermic reaction sufficiency of the corresponding infiltration reaction area.
[0099] In another embodiment of the present application, the number of exothermic reaction pixels is taken as the exponent of an exponential function with a natural constant as the base, and the product of the calculation result of the exponential function and the increase in the neighborhood temperature is taken as the degree of exothermic reaction in the infiltration reaction area.
[0100] In other embodiments of the present application, the sum of the number of exothermic reaction pixels and the increase in neighborhood temperature can also be used as the degree of exothermic reaction sufficiency in the infiltration reaction area.
[0101] A5, based on the degree of exothermic reaction of each infiltration reaction area at all sampling moments, predict the predicted value of the degree of exothermic reaction at the next sampling moment; combine the prediction results of all infiltration reaction areas at the next sampling moment for several consecutive times to adjust the reaction infiltration time.
[0102] In the reactive infiltration process, when all the infiltration reaction areas have undergone sufficient Si-C reaction to form a high-density Si-C matrix, the reactive infiltration heating should be stopped in time to prevent the reactive infiltration time from being too long, causing a large amount of thermal damage to the fibers, which greatly affects the mechanical properties of silicon carbide ceramic-based composites.
[0103] According to the above analysis, the degree of exothermic reaction sufficiency of any infiltration reaction area at all sampling moments is obtained, and the results are sorted in ascending time order as the exothermic reaction sufficiency sequence of the infiltration reaction area. The exothermic reaction sufficiency sequence of each infiltration reaction area is predicted by the Holt linear trend method, wherein the smoothing coefficient and trend coefficient of the Holt linear trend method can be obtained by the cross-validation method, and the predicted value of the degree of exothermic reaction sufficiency of each corresponding infiltration reaction area at the next sampling moment is output. Among them, the Holt linear trend method is a well-known technology and will not be repeated here. In other embodiments of the present application, the predicted value of the degree of exothermic reaction sufficiency at the next sampling moment can also be predicted by an autoregressive model, a moving average method, etc.
[0104] Calculate the predicted exothermic reaction degree of the current reaction infiltration process based on the predicted value of the exothermic reaction sufficiency of all infiltration reaction areas at the next acquisition time , specifically: ; is the predicted exothermic reaction extent of the current reactive infiltration process, is the predicted value of the exothermic reaction sufficiency of the j-th infiltration reaction zone, and Norm() is the normalization function.
[0105] It should be understood that the greater the predicted degree of exothermic reaction, the more intense the reaction of the Si-C system in the infiltration reaction area, the sufficient carbon source in the preform, and the rapid formation of the Si-C matrix on the preform. In order to ensure that the Si melt fully fills the pores inside the preform and Si reacts fully with carbon, the heating of the reaction infiltration process cannot be stopped.
[0106] The present application pre-sets a predicted reaction threshold value. When the predicted exothermic reaction degree of the reactive melt infiltration process is lower than the preset predicted reaction threshold value for a preset number of consecutive times, it means that the Si-C system reaction carried out by the reactive melt infiltration process has been sufficient, and there is no need to carry out reactive melt infiltration process heating to avoid a large amount of thermal damage to the fiber; otherwise, the reactive melt infiltration process heating is continued, wherein the predicted reaction threshold value in this embodiment is 0.3, and the preset number of times is 5.
[0107] The three-point bending strength test of the water-resistant silicon carbide ceramic matrix composite material was carried out at room temperature. The bending stress-displacement curve and tensile stress-displacement curve of the water-resistant silicon carbide ceramic matrix composite material are shown in the attached figure. Figure 7 and attached Figure 8 shown.
[0108] In the attached Figure 7 The horizontal axis is displacement, the unit is millimeter (mm), and the vertical axis is bending stress, the unit is (MPa). Figure 8 The horizontal axis is displacement in millimeters (mm), and the vertical axis is tensile stress in MPa.
[0109] Embodiment 2:
[0110] In Example 2, during the mixed ball milling process, yttrium oxide powder, silicon carbide powder, polyvinyl alcohol and solvent were mixed in a mass ratio of 40:10:12:50; the solvent was a combination of ethanol and xylene.
[0111] Except for the different mass ratio of raw materials in the mixing ball milling process, other parts in Example 2 are the same as those in Example 1.
[0112] Embodiment 3:
[0113] In Example 3, during the mixed ball milling process, yttrium oxide powder, silicon carbide powder, polyvinyl alcohol and solvent were mixed in a mass ratio of 30:6:15:35; the solvent was a combination of ethanol, isopropanol and xylene.
[0114] Except for the different mass ratio of raw materials in the mixed ball milling process, other parts in Example 3 are the same as those in Example 1.
[0115] The various embodiments in the present application are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0116] It should be noted that, unless otherwise specified and limited, terms such as "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that a circuit structure, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such article or device. In the absence of further restrictions, an element defined by the sentence "including one..." does not exclude the existence of other identical elements in the article or device including the element. In addition, the term "and\or" used herein includes any and all combinations of one or more related listed items.
[0117] Those skilled in the art will readily appreciate other embodiments of the present application after considering the specification and practicing the invention herein. The present application is intended to cover any variations, uses or adaptations of the present application, which follow the general principles of the present application and include common knowledge or customary technical means in the art that are not invented by the present application.
[0118] It should be understood that the present application is not limited to the exact construction that has been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof.
Claims
1. An intelligent preparation method for water-resistant silicon carbide ceramic-based composite materials, It is characterized in that The method comprises the following steps: Mixing and ball-milling yttrium oxide powder, silicon carbide powder, polyvinyl alcohol and solvent according to a preset mass ratio to obtain a mixed slurry; The silicon carbide fibers are braided and cut to obtain a first silicon carbide fiber preform, and boron nitride and silicon carbide are deposited to obtain a second silicon carbide fiber preform; The second silicon carbide fiber preform is impregnated in the mixed slurry to obtain an impregnated preform; the impregnated preform is subjected to cutting, lamination, drying, curing, and primary pyrolysis in sequence to obtain a fiber preform; The fiber preform is impregnated in a phenolic resin, and then subjected to secondary pyrolysis and reactive infiltration to obtain a water- and oxygen-resistant silicon carbide ceramic-based composite material. During the reactive infiltration process, the control process of the reactive infiltration time is specifically as follows: A1, obtain the infiltration working temperature diagram at each acquisition moment; A2, based on the temperature diffusion decrease of any pixel in the local temperature neighborhood and the increase of the neighborhood temperature, obtain the exothermic reaction pixel suspicion of any pixel; A3, based on the difference in the suspected degrees of all exothermic reaction pixels in the infiltration condition temperature map within a preset acquisition period between pixels, the infiltration reaction area in the infiltration condition temperature map is screened out; A4, based on the number of pixels corresponding to the exothermic reaction pixel suspicion degree that meets the threshold condition in each infiltration reaction area and the increase in the neighborhood temperature of all pixels in each infiltration reaction area, determine the degree of exothermic reaction sufficiency of each infiltration reaction area; A5, based on the degree of exothermic reaction of each infiltration reaction area at all sampling moments, predict the predicted value of the degree of exothermic reaction at the next sampling moment; combine the prediction results of all infiltration reaction areas at the next sampling moment for several consecutive times to adjust the reaction infiltration time.
2. An intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material as claimed in claim 1, It is characterized in that The yttrium oxide powder, silicon carbide powder, polyvinyl alcohol and solvent in the mixed ball mill are mixed according to the mass ratio of (20-40):(1-10):(7-15):(35-50).
3. An intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material as claimed in claim 2, It is characterized in that The solvent is one or a combination of ethanol, isopropanol or xylene.
4. The intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material according to claim 1, It is characterized in that The obtaining of the second silicon carbide fiber preform further comprises: depositing boron nitride on the first silicon carbide fiber preform to obtain a BN interface layer; and depositing silicon carbide on the basis of the BN interface layer to obtain the second silicon carbide fiber preform.
5. An intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material as claimed in claim 4, It is characterized in that The specific deposition parameters of the BN interface layer when depositing boron nitride are as follows: boron trichloride is used as the boron source, ammonia is used as the nitrogen source, hydrogen is used as the dilution gas, the deposition temperature is set to 700ºC, and the deposition pressure is set to 5kPa; the specific deposition parameters of the second silicon carbide fiber preform when depositing silicon carbide are as follows: trichloromethylsilane is used as the gaseous precursor, hydrogen is used as the carrier gas, argon is used as the dilution gas, the deposition temperature is 1100°C, and the deposition pressure is 5kPa.
6. The intelligent preparation method of the water-oxidation-resistant silicon carbide ceramic-based composite material according to claim 1, It is characterized in that The process of obtaining the impregnated preform is to perform pressure impregnation and vacuum impregnation in the mixed slurry in sequence.
7. The intelligent preparation method of the water-oxidation-resistant silicon carbide ceramic matrix composite material according to claim 1, It is characterized in that The method for determining the exothermic reaction pixel suspiciousness comprises: For each pixel in the local temperature neighborhood with any pixel as the central pixel, count the step length from each pixel to the central pixel, and take the pixels with the same step length as the same circle pixels; arrange them from small to large in order, and form the same circle pixels with the same step length into each circle pixel; Calculate the difference in the temperature mean between adjacent circle pixels, and take the cumulative sum of the differences between all adjacent circle pixels in the local temperature neighborhood of the central pixel as the temperature diffusion decrease of the central pixel in the local temperature neighborhood; wherein the difference is the difference between the temperature mean of the circle with a small step size and the circle with a large step size in the adjacent circle pixels; The difference between the temperature mean of the pixels in the local temperature neighborhood of the central pixel and the temperature mean of the pixels in the infiltration working condition temperature map to which it belongs is taken as the increase of the neighborhood temperature of the central pixel in the local temperature neighborhood; The product of the temperature diffusion decrease and the neighborhood temperature increase is taken as the exothermic reaction pixel suspicion of the central pixel.
8. An intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material as claimed in claim 7, It is characterized in that The screening process of the infiltration reaction area includes: Calculate the cumulative sum of the exothermic reaction pixel suspicion of any pixel in the infiltration working condition temperature map within the preset acquisition period as the exothermic reaction credibility of any pixel; The exothermic reaction credibility of each pixel is used to replace the temperature value of the corresponding pixel in the infiltration working condition temperature map, and the result after replacement is used as the exothermic reaction credibility map; the exothermic reaction credibility map is segmented into superpixels to obtain a number of superpixel blocks; Calculate the exothermic reaction credibility mean of all pixels in each superpixel block; perform threshold segmentation on the exothermic reaction credibility mean of all superpixel blocks, output the credible threshold, and correspond the superpixel blocks whose exothermic reaction credibility mean is greater than or equal to the credible threshold to the area in the infiltration industrial control temperature map, which is recorded as the infiltration reaction area.
9. An intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material as claimed in claim 8, It is characterized in that The method for determining the degree of sufficiency of the exothermic reaction comprises: The exothermic reaction pixel suspicion of all pixels in the infiltration working condition temperature map at any acquisition time is segmented by threshold, and the suspicion threshold is output, and the pixels whose exothermic reaction pixel suspicion is greater than or equal to the suspicion threshold are regarded as exothermic reaction pixels; the number of exothermic reaction pixels in any infiltration reaction area is counted; Calculate the average value of the neighborhood temperature increase of all pixels in any infiltration reaction area at any acquisition moment; The number of exothermic reaction pixels and the average value of the neighborhood temperature increase are combined to obtain the degree of sufficiency of the exothermic reaction.
10. An intelligent preparation method of a water-oxidation-resistant silicon carbide ceramic-based composite material according to claim 9, It is characterized in that Based on the exothermic reaction sufficiency of each infiltration reaction area at all sampling moments, the predicted value of the exothermic reaction sufficiency at the next sampling moment is predicted; and the reaction infiltration time is regulated by combining the prediction results of all the infiltration reaction areas at the next sampling moment for several consecutive times, specifically: The exothermic reaction sufficiency of any infiltration reaction region at all sampling moments is used to form an exothermic reaction sufficiency sequence of the corresponding infiltration reaction region; Predicting the predicted value of the exothermic reaction sufficiency of the exothermic reaction sufficiency sequence of each infiltration reaction area at the next acquisition moment; The normalized value of the cumulative sum of the predicted values of the exothermic reaction sufficiency of all infiltration reaction areas at the next acquisition moment is used as the predicted exothermic reaction degree of the current reactive infiltration process; If the predicted exothermic reaction degree of the reactive infiltration process is lower than a preset predicted reaction threshold value for a consecutive preset number of times, the heating of the reactive infiltration process is stopped.