Antiperovskite structure semiconductor material, X-ray detector and preparation method thereof
Through the combination of anti-perovskite structure semiconductor materials and cementitious material modification layers, the problems of existing X-ray detector materials being easily corroded in the air and low sensitivity are solved, and high-stability and high-sensitivity X-ray detection is achieved. device, suitable for commercial production.
Patent Information
- Application Number
- CN202411019977.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The semiconductor materials of existing X-ray detectors have low atomic numbers, resulting in low X-ray absorption capabilities, difficulty in device preparation, and easy damage. In addition, organic-inorganic hybrid materials are easily corroded by water and oxygen in the air, resulting in insufficient sensitivity and lower detection limits. .
Semiconductor material using anti-perovskite structure (general chemical formula: (2-Habch)3(AI6)B, where 2-Habch is 2-azabicyclo[2,2,1]heptane, and A is a tetravalent metal Such as platinum or tellurium, B is a monovalent halogen such as chlorine or iodine. The X-ray detector is prepared by polishing, coating and thermal evaporation methods, combined with a gel material modification layer and a spacer metal electrode.
It achieves long-term stability in the air environment, improves the product of carrier mobility and carrier lifetime, improves sensitivity and lower detection limit, simplifies the preparation process, and is suitable for commercial production.
Smart Images

Figure CN118546178B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor materials, and in particular relates to an antiperovskite structure semiconductor material, an X-ray detector and a preparation method thereof. Background Art
[0002] X-ray detection is one of the main technologies in non-destructive detection. It can be used in medical testing, industrial flaw detection, safety inspection and other fields that require non-destructive testing.
[0003] The semiconductor materials currently used in commercial X-ray detectors are mainly inorganic materials such as single crystal silicon, amorphous selenium, and cadmium zinc telluride. However, due to their relatively small atomic numbers, their X-ray absorption coefficients are small. In addition, single crystal silicon devices are difficult to prepare and are easily damaged. Amorphous selenium is an amorphous material with a small product of carrier mobility and carrier lifetime, low sensitivity, high detection limit, and is not sensitive enough to X-rays. The preparation process of this type of semiconductor material is relatively cumbersome and the preparation conditions are harsh, which makes it difficult to combine it with a substrate to prepare an X-ray detector.
[0004] In view of this, the research on semiconductor materials for X-ray detectors tends to be in the direction of organic-inorganic hybrid materials. Among them, organic-inorganic hybrid perovskites can promote the absorption of high-energy X-rays due to their heavy atoms with high atomic coefficients. X-ray detectors made of this semiconductor material have a series of advantages such as high X-ray attenuation coefficient, large product of carrier mobility and carrier lifetime, high defect tolerance, and solution processing. However, due to the properties of organic-inorganic hybrid semiconductor materials themselves, they are easily corroded by water and oxygen in the air and are difficult to use stably for a long time; in addition, they also have defects such as low sensitivity and low detection limit. Summary of the invention
[0005] In view of this, the present invention aims to provide an antiperovskite structured semiconductor material, an X-ray detector and a method for preparing the same, aiming to solve at least one technical problem in the background technology.
[0006] The present invention is achieved in that:
[0007] The first aspect of the present invention provides an antiperovskite structure semiconductor material, wherein the antiperovskite structure semiconductor material has the following general chemical formula: (2-Habch)3(AI6)B;
[0008] Wherein, 2-Habch is 2-azabicyclo[2,2,1]heptane; A is a tetravalent metal; and B is a monovalent halogen.
[0009] Furthermore, the tetravalent metal is platinum or tellurium.
[0010] Furthermore, the monovalent halogen is chlorine or iodine.
[0011] Furthermore, the chemical formula of the semiconductor material with an antiperovskite structure is (2-Habch)3(PtI6)Cl or (2-Habch)3(TeI6)I, preferably (2-Habch)3(PtI6)Cl.
[0012] A second aspect of the present invention provides an X-ray detector comprising the above-mentioned antiperovskite structured semiconductor material.
[0013] Furthermore, the X-ray detector comprises a modification layer, a semiconductor layer and an electrode which are stacked in sequence from bottom to top; the material of the semiconductor layer adopts the semiconductor material of the antiperovskite structure, and the semiconductor layer is the core layer of the X-ray detector.
[0014] Furthermore, the modification layer adopts a gelling material with extended functions, such as polymethyl methacrylate, poly (9-vinyl carbazole), polyacrylic acid, polyvinyl pyrrolidone, organic silica gel, epoxy resin, anaerobic glue, hot melt adhesive, pressure sensitive adhesive, latex, etc.
[0015] Furthermore, the electrodes are two sets of spaced metal electrodes, such as gold, silver, copper, etc.
[0016] A third aspect of the present invention provides a method for preparing the above-mentioned X-ray detector, comprising the following steps:
[0017] Polishing the surface of the semiconductor material with an antiperovskite structure to prepare a semiconductor layer;
[0018] forming a modified layer on the bottom of the semiconductor layer by a coating method;
[0019] A planar electrode is deposited on top of the semiconductor layer by thermal evaporation.
[0020] Furthermore, the modification layer is made of gelling material; and the electrodes are two sets of spaced metal electrodes.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention designs a semiconductor material with an antiperovskite structure, which can remain stable for a long time in an air environment, is not easily corroded by water and oxygen in the air, and has excellent stability.
[0023] 2. The X-ray detector made of the semiconductor material with the antiperovskite structure of the present invention has the advantages of high μτ and high sensitivity.
[0024] 3. The X-ray detector made of the semiconductor material with an antiperovskite structure of the present invention can still reflect the current signal generated by X-ray irradiation under low bias voltage and low X-ray dose rate, and has a low detection limit.
[0025] 4. The X-ray detector made of the semiconductor material with an antiperovskite structure of the present invention can be conveniently combined with other X-ray detectors by utilizing the scalability of its modified layer.
[0026] 5. The preparation process of the X-ray detector of the present invention is simple and can be applied to commercial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a structural schematic diagram of the X-ray detector in the present invention;
[0028] Figure 2 The actual X-ray diffraction pattern and the simulated X-ray diffraction pattern of the antiperovskite structure semiconductor material (2-Habch)3(PtI6)Cl prepared in Example 1;
[0029] Figure 3 The actual X-ray diffraction pattern and the simulated X-ray diffraction pattern of the antiperovskite structure semiconductor material (2-Habch)3(TeI6)I prepared in Example 2;
[0030] Figure 4 The current density-time curve diagram of the X-ray detector prepared in Example 3 under different bias voltages;
[0031] Figure 5 The current density-time diagram of the X-ray detector prepared in Example 3 at different bias voltages and different dose rates;
[0032] Figure 6 This is a current-voltage curve diagram of the X-ray detector prepared in Example 3;
[0033] Figure 7 The current density-time curve diagram of the X-ray detector prepared in Example 4 under different bias voltages;
[0034] Figure 8 The current density-time diagram of the X-ray detector prepared in Example 4 at different bias voltages and different dose rates;
[0035] Fig. 9 is a current-voltage curve diagram of the X-ray detector prepared in Example 4;
[0036] Fig.10 The XRD spectrum of the antiperovskite structure semiconductor material (2-Habch)3(PtI6)Cl prepared in Example 1 after aging in an air environment;
[0037] Fig.11 This is a dose rate-signal-to-noise ratio relationship diagram of the X-ray detector prepared in Example 3;
[0038] Fig.12 This is a dose rate-signal-to-noise ratio relationship diagram of the X-ray detector prepared in Example 4. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] The present invention designs a semiconductor material with an antiperovskite structure, whose general chemical formula is (2-Habch)3(AI6)B; wherein 2-Habch is 2-azabicyclo[2,2,1]heptane; A is a tetravalent metal, such as platinum or tellurium; and B is a monovalent halogen, such as chlorine or iodine.
[0041] The present invention prepares an X-ray detector based on the above-mentioned antiperovskite structure semiconductor material, and the preparation steps are: firstly, the surface of the antiperovskite structure semiconductor material (2-Habch)3(Al6)B is polished to prepare a semiconductor layer; a modified layer is formed on the bottom of the semiconductor layer by a coating method; a planar electrode is deposited on the upper part of the semiconductor layer by a thermal evaporation method, and the obtained X-ray detector structure is as follows Figure 1 As shown, it includes a modification layer 1, a semiconductor layer 2 and an electrode 3 which are stacked in sequence from bottom to top.
[0042] The modification layer 1 is made of a gelling material, which has an expansion function, thereby improving the scalability of the device and facilitating the combination with other X-ray detectors. The modification layer 1 can be made of any gelling material permitted in the art, including but not limited to polymethyl methacrylate, poly(9-vinylcarbazole), polyacrylic acid, polyvinyl pyrrolidone, organic silica gel, epoxy resin, anaerobic glue, hot melt adhesive, pressure sensitive adhesive, latex, etc. In the following embodiments, polymethyl methacrylate and organic silica gel are selected as examples, but are not limited to these materials, and other gelling materials not listed are also applicable.
[0043] The electrode 3 uses two sets of spaced metal electrodes. The materials used for the metal electrodes include but are not limited to gold, silver, and copper. In the following embodiments, gold electrodes are selected as examples, but are not limited to this material. Other metal electrode materials not listed are also applicable.
[0044] Example 1
[0045] In this embodiment, the semiconductor material (2-Habch)3(PtI6)Cl with an antiperovskite structure is prepared by the following steps:
[0046] (1) Dissolve 2 mmol of platinum tetrachloride in 30 mL of a mixed solvent consisting of methanol and acetonitrile, where the volume of methanol: the volume of acetonitrile is 1:2, and then add 14 mmol of lithium iodide and stir well to obtain a clear solution;
[0047] (2) Dissolve 6 mmol of 2-azabicyclo[2,2,1]heptane (2-Habch) in the solution prepared in step (1), and slowly evaporate the solution to obtain black crystals.
[0048] Depend on Figure 2 The actual X-ray diffraction pattern and the simulated X-ray diffraction pattern confirmed that the crystal structure was (2-Habch)3(PtI6)Cl. Figure 2 The actual X-ray diffraction pattern uses Cu Kα radiation and sets λ=1.54Å.
[0049] Example 2
[0050] In this embodiment, the semiconductor material (2-Habch)3(TeI6)I with an antiperovskite structure is prepared in the following steps:
[0051] (1) Dissolve 12 mmol of tellurium dioxide in about 82 mmol of hydroiodic acid aqueous solution (concentration 57%) at room temperature;
[0052] (2) Mix 15 mmol of 2-azabicyclo[2,2,1]heptane (2-Habch) with 30 mmol of aqueous hydroiodic acid (concentration 57%);
[0053] (3) The two solutions prepared in step (1) and step (2) are mixed and reacted, and a dark precipitate appears immediately; the precipitate is collected by filtration and washed with toluene;
[0054] (4) Dissolve the precipitate in N,N-dimethylformamide and transfer it to an evaporating dish. Evaporate the solution in the evaporating dish at room temperature. After a few days, dark, shiny cubic crystals are collected.
[0055] Depend on Figure 3 The actual X-ray diffraction pattern and the simulated X-ray diffraction pattern confirmed that the crystal structure was (2-Habch)3(PtI6)Cl. Figure 3 The actual X-ray diffraction pattern uses Cu Kα radiation and sets λ=1.54Å.
[0056] Example 3
[0057] In this embodiment, an X-ray detector is prepared based on the semiconductor material (2-Habch)3(PtI6)Cl with an antiperovskite structure obtained in Example 1, and the steps are as follows:
[0058] S1. Polish the surface of the black crystal (2-Habch)3(PtI6)Cl using 8000-grit sandpaper to form a semiconductor layer;
[0059] S2, dissolving polymethyl methacrylate in toluene to prepare a 40 mg / mL gel solution, applying the solution to the bottom of the semiconductor layer, and forming a modified layer after drying;
[0060] S3, placing the sample obtained in step S2 in a vacuum coating machine at 2×10 -4 Under a pressure of 1.3 Pa, two sets of planar gold electrodes were deposited on the upper surface of the semiconductor layer by thermal evaporation through a mask. The thickness of the gold electrodes was 100 nm and the distance between the two sets of gold electrodes was 0.05 mm, thus obtaining an X-ray detector.
[0061] The current density-time curves of the X-ray detector prepared in this embodiment under different bias voltages are shown in FIG. Figure 4 As shown, the current density-time diagram of the X-ray detector under different bias voltages and different dose rates is as follows Figure 5 As shown, the current-voltage curve of the X-ray detector is as follows Figure 6 As shown, the Hecht equation is substituted to fit the obtained current-voltage curve, and the carrier mobility and carrier lifetime (μτ) values are calculated.
[0062] Calculation shows that the X-ray detector μτ=6.25×10 -3 cm 2 V -1 ; Sensitivity is 10122.8µC Gy air -1 cm -2 In addition, Figure 4 and Figure 5 It can be seen that under low bias voltage, the X-ray detector manufactured in this embodiment can detect the current signal generated by X-ray irradiation.
[0063] Example 4
[0064] This embodiment prepares an X-ray detector based on the semiconductor material (2-Habch)3(TeI6)I with an antiperovskite structure obtained in Example 2, and the steps are as follows:
[0065] S1. Polishing the surface of the antiperovskite structure semiconductor material (2-Habch)3(TeI6)I using 8000-grit sandpaper to obtain a semiconductor layer;
[0066] S2, coating the organic silica gel evenly on the bottom of the semiconductor layer to form a modified layer after drying;
[0067] S3, placing the sample obtained in step S2 in a vacuum coating machine at 2×10-4 Under a pressure of 1.3 Pa, two sets of planar gold electrodes were deposited on the upper surface of the semiconductor layer by thermal evaporation through a mask. The thickness of the gold electrodes was 100 nm and the distance between the two sets of gold electrodes was 0.05 mm, thus obtaining an X-ray detector.
[0068] The current density-time curves of the X-ray detector prepared in this embodiment under different bias voltages are shown in FIG. Figure 7 As shown, the current density-time diagram of the X-ray detector under different bias voltages and different dose rates is as follows Figure 8 As shown, the current-voltage curve of the X-ray detector is as follows Fig. 9 As shown, the Hecht equation is substituted to fit the obtained current-voltage curve, and the carrier mobility and carrier lifetime (μτ) values are calculated.
[0069] Calculation shows that the X-ray detector μτ=4.36×10 -5 cm 2 V -1 ; Sensitivity is 380.8µC Gy air -1 cm -2 .Depend on Figure 7 and Figure 8 It can be seen that under low bias voltage, the X-ray detector manufactured in this embodiment can still detect the current signal generated by X-ray irradiation.
[0070] Comparative Example 1
[0071] This comparative example is a commercial direct-type X-ray detector based on single-crystal silicon as a semiconductor layer.
[0072] Comparative Example 2
[0073] This comparative example is a commercial direct X-ray detector based on amorphous selenium as a semiconductor layer.
[0074] Comparative Example 3
[0075] This comparative example is a commercial direct X-ray detector based on cadmium zinc telluride as a semiconductor layer.
[0076] The test parameters of the X-ray detectors prepared in the above-mentioned Examples 3 and 4 were compared with the test parameters of the commercial X-ray detectors of Comparative Examples 1 to 3, and the results are shown in Table 1.
[0077] Table 1
[0078]
[0079] Note: The sensitivity data are obtained when the voltage is tested at -1V.
[0080] Both μτ and sensitivity can reflect the performance of the X-ray detector. The larger the values of μτ and sensitivity, the better the performance of the X-ray detector. From the values in Table 1, it can be seen that Example 1 exhibits excellent X-ray detection performance, and the sensitivity of the X-ray detector prepared in Example 2 is also better than that of Comparative Examples 1 to 3. It can be seen that the X-ray detector made of antiperovskite structure semiconductor materials of the present invention has better performance than some commercialized X-ray detectors; among them, the X-ray detector made of (2-Habch)3(PtI6)Cl as a semiconductor material in Example 1 has the best performance.
[0081] The antiperovskite structure semiconductor material (2-Habch)3(PtI6)Cl prepared in Example 1 was processed into a thin film, and then an aging test was performed in air. Specifically, the XRD spectrum of the film after aging in air for 18 days, 25 days, 35 days, and 50 days was analyzed, and the XRD spectrum was compared with the XRD spectrum of the freshly prepared film. The results are as follows: Fig.10 As shown, it can be seen that (2-Habch)3(PtI6)Cl has basically no change after aging in air environment for 50 days, that is, it can remain stable in air for a long time.
[0082] The relationship between the dose rate and the signal-to-noise ratio of the X-ray detectors prepared in Example 3 and Example 4 is as follows: Fig.11 and Fig.12 As shown in the results, the detection limit of the X-ray detector prepared in Example 3 is 0.13nGy air s -1 The detection limit of the X-ray detector prepared in Example 4 is 3.08nGy air s -1 ; X-ray detectors made of several common perovskite structure semiconductor materials on the market were purchased, and their detection limits were compared with those of Example 3 and Example 4 of the present invention. The results are shown in Table 2.
[0083] Table 2
[0084]
[0085] Note: The semiconductor in perovskite X-ray detector 1 is a perovskite MAPbI3 single crystal; the semiconductor in perovskite X-ray detector 2 is a perovskite MAPbBr3 single crystal; the semiconductor in perovskite X-ray detector 3 is a thin film prepared by the perovskite CsPbBr3 solution method; the semiconductor in perovskite X-ray detector 4 is a thin film prepared by the perovskite CsPbI3 hot pressing method.
[0086] It can be seen from Table 2 that the detection limit of the X-ray detector prepared in Example 3 is much lower than that of the conventional perovskite X-ray detector.
[0087] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An antiperovskite structured semiconductor material, characterized in that: The semiconductor material of the antiperovskite structure has the following general chemical formula: (2-Habch)3(AI6)B; Wherein, 2-Habch is 2-azabicyclo[2,2,1]heptane; A is platinum or tellurium; and B is a monovalent halogen.
2. The semiconductor material of the antiperovskite structure according to claim 1, characterized in that: The monovalent halogen is chlorine or iodine.
3. The semiconductor material of the antiperovskite structure according to claim 1, characterized in that: The chemical formula of the antiperovskite structured semiconductor material is (2-Habch)3(PtI6)Cl or (2-Habch)3(TeI6)I.
4. X-ray detector, characterized in that The X-ray detector comprises the antiperovskite structure semiconductor material according to any one of claims 1 to 3.
5. The X-ray detector according to claim 4, characterized in that: The X-ray detector comprises a modification layer, a semiconductor layer and an electrode which are stacked in sequence from bottom to top; the material of the semiconductor layer adopts the semiconductor material of the antiperovskite structure.
6. The X-ray detector according to claim 5, characterized in that: The finishing layer is made of gelling material.
7. The X-ray detector according to claim 5, characterized in that: The electrodes are two sets of spaced metal electrodes.
8. A method for preparing an X-ray detector, characterized in that: The preparation method is used to prepare the X-ray detector according to any one of claims 4 to 7, and the preparation method comprises the following steps: Polishing the surface of the semiconductor material with an antiperovskite structure to prepare a semiconductor layer; forming a modified layer on the bottom of the semiconductor layer by a coating method; A planar electrode is deposited on top of the semiconductor layer by thermal evaporation.