A method and carrier for preparing microcarriers for cell cultured meat production based on a novel low-temperature induced phase separation technology

By using a new low-temperature-induced phase separation technology in the preparation of microcarriers, the emulsion is directly poured into the pre-cooled phase separation liquid for stirring, and washed with a similar phase separation liquid, which solves the problem of uneven heat transfer rate and emulsion particles. The problem of adhesion and food safety risks has been eliminated, and efficient and safe microcarrier preparation has been achieved.

CN118546869BActive Publication Date: 2024-10-22CHINA MEAT RES CENT
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411014798.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-22
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

In the preparation process of existing microcarriers, there are problems such as unstable heat transfer rate, poor dispersion of emulsion particles, and high food safety risks. Especially in the low-temperature induction method, the emulsion system is prone to adhesion in a low-temperature environment, which affects the physical and chemical properties and production of microcarriers. rate, and poor solvents and pH induction methods have food safety hazards.

Method used

Using new low-temperature induced phase separation technology, by directly adding w/o emulsion into the pre-cooled phase separation liquid and stirring, it ensures that the emulsion particles phase separate at the same time, reduces the probability of adhesion, and uses a phase separation liquid similar to the oil phase solvent. Washing is performed to quickly complete the phase separation process to ensure the dispersion and edibleability of the microcarriers.

Benefits of technology

It achieves the preparation of microcarriers with high dispersion of emulsion particles, no difference in phase separation time, and high food safety, reduces preparation time and cost, and improves the physical and chemical properties and edibility of microcarriers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118546869B_ABST
    Figure CN118546869B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of cell cultured meat, and in particular to a method and carrier for preparing microcarriers for cell cultured meat production based on a novel low-temperature induced phase separation technology. Based on the novel low-temperature induced phase separation technology, the method comprises mixing a raw material aqueous solution and an oil phase solvent, adding a crosslinking agent and an emulsifier to obtain an emulsion, precooling the phase separation liquid and then adding the emulsion, and filtering and freeze-drying. The defects of unstable heat transfer rate, poor dispersion of emulsion particles, and high food safety risks are solved, and microcarriers for cell cultured meat production are quickly prepared. The preparation method of the present invention has the beneficial effects of high dispersion of emulsion particles, no difference in phase separation time, and high food safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of cell cultured meat, and in particular relates to a method and a carrier for preparing microcarriers for cell cultured meat production based on a novel low-temperature induced phase separation technology, which is obtained based on the novel low-temperature induced phase separation technology. Background Art

[0002] The production of cell-cultured meat mainly includes the following four key steps: obtaining seed cells, developing serum-free culture medium, large-scale cell expansion and differentiation, and food safety assessment. Among them, in the large-scale cell expansion and differentiation stage, it is necessary to use a large bioreactor to expand the seed cells. However, most of the cells used in the production process can only proliferate in a wall-attached state, and the bioreactor cannot provide a place for cells to adhere to the wall. Therefore, it is necessary to add microcarriers to the bioreactor so that the cells can attach to the surface of the microcarriers to complete subsequent proliferation.

[0003] Microcarriers are mainly microspheres with a diameter of 200 to 300 microns, and their synthesis methods mostly use the emulsion method. The specific process is to first mix a certain concentration of raw material aqueous solution with a hydrophobic solvent in a certain proportion, add an emulsifier and a cross-linking agent, and obtain a w / o type emulsion (oil-in-water type emulsion) after a certain period of reaction; then separate the aqueous phase from the emulsion system through a certain phase separation method (commonly known as demulsification); finally, select a matching post-treatment method according to the phase separation method to obtain the microcarrier product. Phase separation itself is a physical and chemical concept, which refers to the phenomenon of adding a poor solvent to the emulsion system or reducing the solubility of the solute by changing the temperature and pH of the system, and condensing from the emulsion system. Existing technical data show that the phase separation step is a key step in the preparation of microcarriers, and the choice of phase separation method has a great influence on the physicochemical properties and biological activity of the microcarriers.

[0004] The existing phase separation methods in the microcarrier preparation process mainly include poor solvent induction method, low temperature induction method and pH induction method, as follows:

[0005] Poor solvent induction method: Adding a poor solvent (such as methanol, ethanol, isopropanol, etc.) to the w / o emulsion (water-in-oil emulsion) system destroys the solubility equilibrium in the emulsion system and causes the water phase solute to precipitate.

[0006] Low-temperature induction method: The entire w / o emulsion (water-in-oil emulsion) system is placed in a low-temperature environment (below 0°C) to destroy the thermodynamic equilibrium of the emulsion system and cause the water phase solute to precipitate.

[0007] Acidity (pH value) induction method: Add a certain amount of acid or alkali to the w / o emulsion (water-in-oil emulsion) system to destroy the solubility equilibrium by changing the acidity (pH value) of the emulsion system, causing the water phase solute to precipitate.

[0008] The technical problems of the above phase separation method are specifically manifested in:

[0009] 1. Poor solvent induction method: Due to the complexity of the emulsion system, it is difficult to determine whether a solvent is a poor solvent. In addition, in most cases, a mixed solvent is required, and the ratio between the components in the mixed solvent requires a long time to explore, and the amount of mixed solvent added also needs to be accurately evaluated. The above steps undoubtedly bring great economic and time costs to the microcarrier preparation process. In addition, since cell culture meat microcarriers must be edible, adding solvents poses a greater food safety risk;

[0010] 2. Low-temperature induction method: This method is the most commonly used phase separation method in the preparation of microcarriers. The specific operation method is to place the obtained emulsion system in a low-temperature environment and freeze it for a certain period of time to allow phase separation to occur. Although this method is simple, it has three defects: ① There is an uneven heat transfer rate between the low-temperature environment and the emulsion system, which cannot guarantee that the entire emulsion system will phase separate at the same time, and the difference in phase separation time will affect the physical and chemical properties and yield of the final harvested microcarriers; ② During the phase separation process of the emulsion system, the emulsion particles are very likely to adhere to each other, and the surface morphology of the adhered emulsion particles is easily destroyed during the post-processing process, thereby affecting the physical and chemical properties of the microcarriers; ③ This method will cause a large amount of oil phase solvent residue in the microcarriers, which will increase the economic and time costs of the post-processing process. At the same time, since the cell cultured meat microcarriers must be edible, the residue of oil phase solvent poses a major food safety hazard;

[0011] 3. Acidity (pH) induction method: Similar to the poor solvent induction method, it is difficult to determine the exact pH value at which the emulsion system undergoes phase separation, and therefore, it is also impossible to accurately assess the amount of acid or base added. In addition, the addition of acid and base will bring greater food safety risks to cell-cultured meat. Summary of the invention

[0012] In order to solve the above technical problems, the present invention provides a method and carrier for preparing microcarriers for cell cultured meat production based on a new low-temperature induced phase separation technology. By improving the traditional emulsion phase separation technology, the phase separation process is optimized based on the new low-temperature induced phase separation technology, which solves the defects of unstable heat transfer rate, poor dispersion of emulsion particles, and high food safety risks. In addition, the low-temperature induced phase separation technology can make the emulsion system phase separate quickly, reduce the time required for the phase separation step, and thus quickly prepare microcarriers for cell cultured meat production. The preparation method has the beneficial effects of high dispersion of emulsion particles, no difference in phase separation time, and high food safety.

[0013] A method for preparing microcarriers for cell cultured meat production based on a novel low-temperature induced phase separation technology in the present invention to solve the above technical problems comprises the following steps:

[0014] (1) Prepare the raw material aqueous solution and the oil phase solvent, and then mix them in a certain proportion;

[0015] (2) adding a crosslinking agent and an emulsifier under stirring or ultrasonic conditions, and reacting for a period of time to obtain a w / o type emulsion (water-in-oil emulsion);

[0016] (3) Preparing a phase separation system: pre-cooling the phase separation liquid in a low-temperature cooling bath for later use;

[0017] (4) Add the w / o type emulsion directly into the pre-cooled phase separation liquid and stir until the phase separation is complete;

[0018] In view of the defect that the traditional low-temperature induction method cannot ensure that the entire emulsion system undergoes phase separation at the same time, the present invention directly pours the emulsion into the pre-cooled phase separation liquid and stirs it, so that each emulsion particle can fully contact with the low-temperature phase separation liquid and undergo phase separation at the same time, thereby ensuring the physical and chemical properties and yield of the microcarriers finally obtained;

[0019] Aiming at the defect that the emulsion system in the traditional low-temperature induction method is prone to adhesion in a static environment, which ultimately affects the physical and chemical properties of the microcarrier, the present invention adopts a strategy of applying stirring during the phase separation process to reduce the probability of mutual adhesion between the emulsion particles and ensure the dispersion of the microcarrier obtained in the end;

[0020] (5) Filter and freeze-dry to obtain microcarrier particles.

[0021] In the optimized solution, the precooling temperature in step (3) is -40°C to -20°C.

[0022] Temperatures above -20°C may reduce the speed of phase separation and fail to achieve the effect of rapid preparation; temperatures below -40°C may cause the phase separation speed to be too fast, leading to adhesion between emulsion particles and affecting the uniformity of the final microcarrier particles.

[0023] In a further optimized solution, the phase separation liquid is petroleum ether; or one of n-pentane, n-hexane and n-heptane; the mass volume ratio of the phase separation liquid to the w / o type emulsion is 4 / 1 to 5 / 1.

[0024] In view of the defects of food safety risks in the three traditional phase separation methods, the phase separation liquid used in the present invention can not only quickly cause phase separation, but also is similarly miscible with the oil phase solvent. The microcarrier particles can be washed while the phase separation process occurs, effectively reducing the residual oil phase solvent and ensuring the edibility of the final microcarriers.

[0025] The raw materials are one or more of chitosan, dextran, gelatin and sodium alginate, and the raw material aqueous solution is a solution prepared by configuring the raw materials into a certain concentration, and the mass fraction of the raw material aqueous solution is 0.01-0.2.

[0026] The oil phase solvent is light paraffin oil, olive oil, toluene, n-hexane and the like.

[0027] The mass volume ratio of the raw material aqueous solution to the oil phase solvent is 0.3 / 1 to 0.5 / 1.

[0028] The emulsifier is Span 80, and the mass volume ratio of the emulsifier to the oil phase solvent is 0.01 / 1 to 0.05 / 1.

[0029] The cross-linking agent is glutaraldehyde, sodium citrate, calcium dichloride, sodium tripolyphosphate, etc. The mass fraction of the aqueous solution of the cross-linking agent is 0.05-0.1; the volume ratio of the cross-linking agent aqueous solution to the oil phase solvent is 0.01 / 1-0.05 / 1.

[0030] In the optimized scheme, the reaction temperature in step (2) is 25-45°C, and the reaction time is 30-60 min; the stirring can be mechanical stirring, and the mechanical stirring speed is 400-600 rpm; or the ultrasonic power is 40 KHz, and the time is 15-20 min.

[0031] In a further optimized solution, in step (4), the speed at which the w / o emulsion is added to the phase separation liquid is 1 to 2 mL / s, and the phase separation time is 30 to 40 min; the stirring is magnetic stirring, and the speed of the magnetic stirring is 1000 to 1500 rpm.

[0032] After phase separation occurs in step (4), stirring for a period of time and replacing the phase separation liquid to repeat this step; starting from the occurrence of phase separation, the phase separation liquid is replaced once every 8 to 10 minutes, and this is continued for 3 to 4 times. Repeating phase separation further reduces the residual oil phase solvent and emulsifier, and the main effect is better.

[0033] In the step (5), the frozen emulsion particles are obtained by vacuum filtration, and then the frozen emulsion particles are placed in a freeze dryer, and the microcarrier particles are obtained after freeze drying; wherein the pore size of the filter paper for vacuum filtration is 15 to 20 μm, the freeze drying temperature is ≤-20°C, the vacuum degree is ≤10 Pa, and the freeze drying time is 24 to 36 h.

[0034] The present invention also provides a carrier prepared by a method for rapidly preparing microcarriers for cell cultured meat production based on the principle of low temperature induced phase separation.

[0035] The present invention overcomes the following technical problems:

[0036] (1) In view of the defect of phase separation time difference caused by uneven heat transfer rate in the traditional low-temperature induction method, the present invention adopts a method of direct contact between the W / O type emulsion and the phase separation liquid to eliminate the phase separation time difference caused by heat transfer rate;

[0037] (2) In view of the defect that the emulsion particles are prone to adhesion in the traditional low-temperature induction method, the present invention will adopt a method of applying stirring or ultrasound during the emulsion cooling process to facilitate the dispersion of the emulsion particles;

[0038] (3) In view of the food safety risks in the three methods of the background technology, the present technical solution will use a phase separation liquid that is similarly miscible with the oil phase solvent to wash the microcarrier particles while the phase separation process is occurring, thereby effectively reducing the residual oil phase solvent and ensuring the edibility of the final microcarrier. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a technical flow chart of the preparation method of the present invention;

[0040] Figure 2 The scanning electron microscope images of the microcarriers prepared in Examples 4 to 6 of the present invention are shown;

[0041] Figure 3 The cell survival rate statistics of the three microcarriers prepared in Examples 4 to 6 of the present invention and chicken myoblasts cultured for three days;

[0042] Figure 4 This is a diagram showing the effect of different phase separation liquid precooling temperatures on the pore size on the microcarrier surface in the present invention;

[0043] Figure 5 The scanning electron microscope photos of the microcarriers prepared by the novel low-temperature induced phase separation technology and the traditional phase separation technology in the present invention;

[0044] Figure 6 The scanning electron microscope photos of the microcarriers obtained with and without stirring during the phase separation process of the present invention are shown. DETAILED DESCRIPTION

[0045] The present invention is further described below in conjunction with specific embodiments:

[0046] like Figure 1 As shown, a method for preparing microcarriers for cell-cultured meat production based on a novel low-temperature induced phase separation technology comprises mixing a raw aqueous solution and an oil phase solvent in a certain proportion, then adding a cross-linking agent and an emulsifier under stirring conditions, and reacting for a period of time to obtain a w / o type emulsion (water-in-oil emulsion); then adding the emulsion to a pre-cooled phase separation liquid, stirring for a period of time, and directly obtaining microcarrier particles through filtration and stirring.

[0047] The specific steps are as shown in the following embodiments:

[0048] Example 1 (1) Prepare a raw material aqueous solution and an oil phase solvent, and mix them in a certain proportion; the raw material aqueous solution is an aqueous solution prepared by configuring the raw material into a certain concentration, the raw material is dextran, and the mass fraction of the raw material aqueous solution is 0.01; the oil phase solvent is olive oil, and the mass volume ratio of the raw material aqueous solution to the oil phase solvent is 0.3 / 1;

[0049] (2) adding a crosslinking agent and an emulsifier under stirring, and reacting for a period of time to obtain a w / o type emulsion; wherein the reaction temperature is 25°C, and the reaction time is 60 min; the stirring can be mechanical stirring, and the mechanical stirring speed is 400 rpm;

[0050] The emulsifier is Span 80, and the volume ratio of the emulsifier to the oil phase solvent is 0.01 / 1; the cross-linking agent is calcium dichloride, and the mass fraction of the cross-linking agent aqueous solution is 0.05; the mass volume ratio of the cross-linking agent aqueous solution to the oil phase solvent is 0.01 / 1;

[0051] (3) Preparing a phase separation system: pre-cooling the phase separation liquid in a low-temperature cooling bath for standby use, the pre-cooling temperature being -35°C; the phase separation liquid is petroleum ether; the mass volume ratio of the phase separation liquid to the w / o emulsion is 4 / 1;

[0052] (4) Add the w / o type emulsion directly into the pre-cooled phase separation liquid and stir until the phase separation is complete; the speed of adding the w / o type emulsion into the phase separation liquid is 1-2 mL / s, and the time for complete phase separation is 30 min; the stirring is magnetic stirring, and the speed of magnetic stirring is 1000 rpm;

[0053] After phase separation occurs, stir for a period of time and replace the phase separation liquid and repeat this step; start timing from the occurrence of phase separation, replace the phase separation liquid once / 8 minutes, and continue for 4 times;

[0054] (5) Filtration and freeze-drying to obtain microcarrier particles:

[0055] The frozen emulsion particles are obtained by vacuum filtration, and then the frozen emulsion particles are placed in a freeze dryer, and the microcarrier particles are obtained after freeze drying; wherein, the pore size of the filter paper for vacuum filtration is 15 μm, the freeze drying temperature is ≤-20°C, the vacuum degree is ≤10Pa, and the freeze drying time is 26 hours.

[0056] Example 2

[0057] (1) preparing a raw material aqueous solution and an oil phase solvent, and then mixing them in a certain proportion; the raw material aqueous solution is an aqueous solution prepared by configuring the raw materials into a certain concentration, the raw material is chitosan, the mass fraction of the raw material aqueous solution is 0.2; the oil phase solvent is toluene, and the mass volume ratio of the raw material aqueous solution to the oil phase solvent is 0.5 / 1;

[0058] (2) adding a crosslinking agent and an emulsifier under stirring, and reacting for a period of time to obtain a w / o type emulsion; wherein the reaction temperature is 45°C, and the reaction time is 30 min; the stirring can be mechanical stirring, and the mechanical stirring speed is 600 rpm;

[0059] The emulsifier is Span 80, and the mass volume ratio of the emulsifier to the oil phase solvent is 0.05 / 1; the cross-linking agent is glutaraldehyde, and the mass fraction of the cross-linking agent aqueous solution is 0.1; the mass volume ratio of the cross-linking agent aqueous solution to the oil phase solvent is 0.05 / 1;

[0060] (3) Preparing a phase separation system: pre-cooling the phase separation liquid in a low-temperature cooling bath for standby use, the pre-cooling temperature being -25°C; the phase separation liquid is n-pentane; the mass volume ratio of the phase separation liquid to the w / o type emulsion is 5 / 1;

[0061] (4) directly adding the w / o type emulsion into the precooled phase separation liquid and stirring until the phase separation is complete; the speed of adding the w / o type emulsion into the phase separation liquid is 1 to 2 mL / s, and the time for the phase separation to be complete is 40 min; the stirring is magnetic stirring, and the speed of the magnetic stirring is 1500 rpm;

[0062] After phase separation occurs, stir for a period of time and replace the phase separation liquid and repeat this step; start timing from the occurrence of phase separation, replace the phase separation liquid once every 10 minutes, and continue for 3 times;

[0063] (5) Filtration and freeze-drying to obtain microcarrier particles:

[0064] The frozen emulsion particles are obtained by vacuum filtration, and then the frozen emulsion particles are placed in a freeze dryer, and the microcarrier particles are obtained after freeze drying; wherein, the pore size of the filter paper for vacuum filtration is 20 μm, the freeze drying temperature is ≤-20°C, the vacuum degree is ≤10 Pa, and the freeze drying time is 32 h.

[0065] Example 3

[0066] (1) preparing a raw material aqueous solution and an oil phase solvent, and then mixing them in a certain proportion; the raw material aqueous solution is an aqueous solution prepared by configuring the raw materials into a certain concentration, the raw material is gelatin, the mass fraction of the raw material aqueous solution is 0.1; the oil phase solvent is n-hexane, and the mass volume ratio of the raw material aqueous solution to the oil phase solvent is 0.4 / 1;

[0067] (2) adding a crosslinking agent and an emulsifier under stirring, and reacting for a period of time to obtain a w / o type emulsion; wherein the reaction temperature is 35°C, and the reaction time is 50 min; the stirring can be mechanical stirring, and the mechanical stirring speed is 450 rpm;

[0068] The emulsifier is Span 80, and the mass volume ratio of the emulsifier to the oil phase solvent is 0.03 / 1; the cross-linking agent is sodium citrate, and the mass fraction of the cross-linking agent aqueous solution is 0.08; the mass volume ratio of the cross-linking agent aqueous solution to the oil phase solvent is 0.03 / 1;

[0069] (3) Preparing a phase separation system: pre-cooling the phase separation liquid in a low-temperature cooling bath for standby use, the pre-cooling temperature being -32°C; the phase separation liquid is n-heptane; the mass volume ratio of the phase separation liquid to the w / o emulsion is 4.5 / 1;

[0070] (4) directly adding the w / o type emulsion into the precooled phase separation liquid and stirring until the phase separation is complete; the speed of adding the w / o type emulsion into the phase separation liquid is 1 to 2 mL / s, and the time for the phase separation to be complete is 35 min; the stirring is magnetic stirring, and the speed of the magnetic stirring is 1200 rpm;

[0071] After phase separation occurs, stir for a period of time and replace the phase separation liquid and repeat this step; start timing from the occurrence of phase separation, replace the phase separation liquid once every 9 minutes, and continue for 3 times;

[0072] (5) Filtration and freeze-drying to obtain microcarrier particles:

[0073] The frozen emulsion particles are obtained by vacuum filtration, and then the frozen emulsion particles are placed in a freeze dryer, and the microcarrier particles are obtained after freeze drying; wherein, the pore size of the filter paper for vacuum filtration is 18 μm, the freeze drying temperature is ≤-20°C, the vacuum degree is ≤10Pa, and the freeze drying time is 30 h.

[0074] Example 4

[0075] (1) Take 1 g of chitosan and add 50 mL of 2% acetic acid solution to prepare a chitosan aqueous solution with a mass fraction of 0.02; mix 20 mL of the chitosan aqueous solution with 40 mL of toluene and add them to a 200 mL three-necked flask and mix well;

[0076] (2) Add 1 mL of Span 80 and 10% sodium citrate or sodium tripolyphosphate solution, and react the entire system at 500 rpm and 30°C for 40 min to form a w / o emulsion;

[0077] (3) While the reaction is going on, prepare 250 mL of petroleum ether and place it in a low-temperature reaction bath to pre-cool it to -40°C.

[0078] (4) After the w / o type emulsion system is stable, the emulsion is added to the phase separation liquid at a rate of 2 mL / s, while the entire system is kept under stirring at a speed of 1000 rpm. After 30 min, the frozen emulsion particles are separated by vacuum filtration, the phase separation liquid is replaced, and the emulsion particles are added to the phase separation liquid again for stirring and washing for 10 min. The above process is repeated 3 times;

[0079] (5) The emulsion particles were separated by vacuum filtration and placed in a freeze dryer with a cold trap temperature of -55 °C and a vacuum degree of 2 to 3 Pa. The emulsion particles were taken out after 36 h to obtain chitosan microcarrier particles.

[0080] Example 5

[0081] (1) Take 10 g of gelatin and add 100 mL of deionized water to prepare a gelatin aqueous solution with a mass fraction of 0.1; mix 20 mL of the gelatin aqueous solution with 40 mL of light paraffin oil or olive oil and add the mixture to a 200 mL three-necked flask;

[0082] (2) Add 0.5 mL of Span 80 and 0.4 mL of 5% glutaraldehyde solution, and react the entire system at 400 rpm and 40°C for 30 min to form a w / o emulsion;

[0083] (3) While the reaction is going on, prepare 200 mL of petroleum ether and place it in a low-temperature reaction bath to pre-cool it to -20°C.

[0084] (4) After the w / o type emulsion system is stable, the emulsion is added to the phase separation liquid at a rate of 2 mL / s, while the entire system is kept under stirring at a speed of 1500 rpm. After 30 min, the frozen emulsion particles are separated by vacuum filtration, the phase separation liquid is replaced, and the emulsion particles are added to the phase separation liquid again for stirring and washing for 10 min. The above process is repeated 3 times;

[0085] (5) The emulsion particles were separated by vacuum filtration and placed in a freeze dryer with a cold trap temperature of -55 °C and a vacuum degree of 2 to 3 Pa. The emulsion particles were taken out after 28 h to obtain gelatin microcarrier particles.

[0086] Example 6

[0087] (1) Take 5 g of sodium alginate and add 50 mL of deionized water to prepare a sodium alginate aqueous solution with a mass fraction of 0.1. Mix 20 mL of chitosan aqueous solution and 40 mL of n-hexane, add them into a 200 mL three-necked flask and mix well.

[0088] (2) Add 0.8 mL of Span 80 and 1 mL of 10% calcium dichloride solution, and react the entire system at 450 rpm and 25 °C for 30 min to form a w / o emulsion;

[0089] (3) While the reaction is going on, prepare 250 mL of petroleum ether and place it in a low-temperature reaction bath to precool it to -30°C.

[0090] (4) After the w / o type emulsion system is stable, the emulsion is added to the phase separation liquid at a rate of 2 mL / s, while the entire system is kept under stirring at a speed of 1500 rpm. After 30 min, the frozen emulsion particles are separated by vacuum filtration, the phase separation liquid is replaced, and the emulsion particles are added to the phase separation liquid again for stirring and washing for 10 min. The above process is repeated 3 times;

[0091] (5) The emulsion particles were separated by vacuum filtration and placed in a freeze dryer with a cold trap temperature of -55 °C and a vacuum degree of 2 to 3 Pa. The emulsion particles were taken out after 24 h to finally obtain sodium alginate microcarrier particles.

[0092] Test 1

[0093] After the samples were completely freeze-dried, 2-3 mg of the three microcarriers in Examples 4-6 were weighed, adhered to the conductive glue, and then sprayed with gold for 2 min under a gold spraying instrument. The three samples were then placed under a scanning electron microscope to observe the particle size and surface morphology of the microcarriers. The results are shown in FIG. Figure 2 shown.

[0094] As attached Figure 2 As shown, Figure 2 1 is a scanning electron microscope photograph of the chitosan-based microcarrier prepared in Example 4, and it can be observed that the particle size is about 200 to 300 microns and the surface is a porous structure; Figure 2 2 is a scanning electron microscope photograph of the gelatin-based microcarrier prepared in Example 4, and it can be observed that the particle size is about 200 to 300 microns, and the surface has relatively fine scaly wrinkles; Figure 2 Figure 3 is a scanning electron microscope photo of the sodium alginate-based microcarrier prepared in Example 6. It can be observed that the particle size is about 300 microns, the shape is ellipsoidal, the surface is rough and there is no pore. It can be seen that a series of microcarriers with different surface morphology characteristics can be prepared using the low temperature induced phase separation technology.

[0095] Test 2

[0096] The cell proliferation kit (CCK-8) was used to characterize the cytotoxicity of the three microcarriers in Examples 4 to 6 in chicken myoblasts. 4 The cells were seeded in a 96-well plate at a density of 10 cells per well. After culturing for 24, 48, and 96 h, the microcarrier dispersion prepared in advance at 2 mg / mL was added to each well. After 2 h of co-culture, 2 μL CCK-8 reagent was added to each well. After incubation at 37°C for 2 h, the absorbance was read using an ELISA reader and the cell survival rate was calculated. The results are shown in Figure 3 shown.

[0097] like Figure 3 As shown, chicken myoblasts were co-cultured with the three microcarriers prepared in Examples 4 to 6 for three days, and the cell survival rate was tested every day. The cell survival rate was higher than 80%, and the cell survival rate increased every day compared with the previous day. On the third day, the cell survival rate was significantly higher than that of the previous two days, indicating that the cells proliferated. The results show that the microcarriers prepared in the present invention have good cell compatibility and no obvious cytotoxicity.

[0098] Test 3

[0099] The other preparation contents are the same, and experimental groups 1, 2 and 3 are set. The precooling temperature of the phase separation liquid in experimental group 1 is minus 40°C, the precooling temperature of the phase separation liquid in experimental group 2 is minus 30°C, and the precooling temperature of the phase separation liquid in experimental group 3 is minus 20°C. See the pore size diagram of the carrier surface. Figure 4 .

[0100] like Figure 4 As shown, the microcarriers prepared by the novel low-temperature induced phase separation technology of the present invention can adjust the pore size on the surface of the microcarriers by adjusting the temperature of the phase separation liquid. As the temperature of the phase separation liquid increases, the diameter of the pores on the surface of the microcarrier (chitosan-based) gradually increases. The regulation of the pore size plays a vital role in maintaining the structural stability of the microcarriers during the subsequent freeze-drying process.

[0101] Test 4

[0102] The other contents are the same, and an experimental group and a control group are set. The experimental group is the preparation method of the present invention, in which the w / o type emulsion is directly added to the pre-cooled phase separation liquid and stirred until the phase separation is complete. The control group is the traditional method in which the entire emulsion system is placed in a low temperature environment, such as a refrigerator or freezer to produce phase separation, as shown in Table 1:

[0103] Table 1 Comparison between the novel low temperature induced phase separation technology of the present invention and the conventional phase separation technology

[0104]

[0105] As shown in Table 1 above, the novel low-temperature induced phase separation technology of the present invention can complete the phase separation step in a shorter time than the traditional method, and since stirring or ultrasound is applied during the process, the dispersion of the emulsion particles is always kept good and not easy to stick. In addition, compared with the traditional method, since the entire phase separation process lasts for a shorter time, the morphology of the microcarrier surface can be regulated according to the temperature of the phase separation liquid.

[0106] Also available from Figure 5 It can be seen that the microcarriers (chitosan-based) prepared by the traditional phase separation method have serious adhesion between particles, and a large number of depressions and voids appear on the surface. These structural defects are not conducive to the subsequent use of the microcarriers. On the other hand, the microcarriers (chitosan-based) prepared by the new low-temperature induced phase separation method have better dispersibility, a porous surface, and no structural defects.

[0107] Test 5

[0108] The other contents are the same, and an experimental group and a control group are set up. The experimental group is stirred during the phase separation process in the preparation method of the present invention.

[0109] The control group was not stirred during the phase separation process. Figure 6 .

[0110] like Figure 6 As shown, it is necessary to apply stirring during the phase separation process. If stirring is not applied, there will be a certain degree of adhesion between the microcarrier particles (chitosan-based) obtained in the end, which will greatly affect the effect of carrier formation.

[0111] Principle of the present invention:

[0112] (1) In the traditional low-temperature induction method, the entire emulsion system is usually placed in a low-temperature environment (refrigerator or freezer) to produce phase separation. However, there is an uneven heat transfer rate between the low-temperature environment and the emulsion system, which cannot ensure that the entire emulsion system undergoes phase separation at the same time. The difference in phase separation time will affect the physical and chemical properties and yield of the final harvested microcarriers. In view of the defects of the traditional low-temperature induction method, in the present invention, the w / o type emulsion is directly poured into the pre-cooled phase separation liquid and stirred, so that each emulsion particle can fully contact with the low-temperature phase separation liquid to cause a phase separation process, eliminating the difference in phase separation time caused by the heat transfer rate, and achieving the purpose of rapidly preparing microcarriers;

[0113] (2) In the traditional low-temperature induction method, the entire emulsion system is usually placed in a low-temperature environment (refrigerator or freezer) to produce phase separation. However, the emulsion system is prone to adhesion in a static environment, and the surface morphology of the adhered emulsion particles is easily destroyed during the post-processing process (freeze drying or vacuum filtration), which ultimately affects the physical and chemical properties of the microcarrier. In the present invention, stirring is applied simultaneously during the phase separation process to reduce the probability of emulsion particles sticking to each other;

[0114] (3) In view of the food safety risks in the three traditional phase separation methods, the phase separation liquid used in the present invention can not only quickly cause phase separation, but also be similarly miscible with the oil phase solvent. During the phase separation process, the microcarrier particles can be washed, effectively reducing the residual oil phase solvent and ensuring the edibility of the microcarriers.

[0115] Since the present invention mainly targets the three defects of the traditional phase separation method, namely (1) the difference in phase separation time caused by uneven heat transfer rate; (2) the easy adhesion of emulsion particles; and (3) the food safety risk, based on the principle of low-temperature induced phase separation, a new phase separation process is redesigned and verified. Therefore, all technologies involved in the phase separation step in the microcarrier preparation process need to be protected. In addition, since the microcarrier preparation scheme involved in the technical solution uses a new phase separation scheme, the entire microcarrier preparation process also needs to be protected.

[0116] The above implementation / test examples are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing microcarriers for cell cultured meat production based on a novel low temperature induced phase separation technology, characterized in that: The following steps are involved: (1) preparing a raw material aqueous solution and an oil phase solvent, and mixing them; the raw material in the raw material aqueous solution is one or more of chitosan, gelatin and sodium alginate; the oil phase solvent is one or more of light paraffin oil, olive oil, toluene and n-hexane; (2) adding a crosslinking agent and an emulsifier under stirring, and obtaining a w / o type emulsion after reaction; the reaction temperature is 25°C to 45°C, and the reaction time is 30 to 60 min; the stirring is mechanical stirring, and the mechanical stirring speed is 400 to 500 rpm; the emulsifier is Span 80, and the crosslinking agent is one or more of glutaraldehyde, sodium citrate, calcium dichloride and sodium tripolyphosphate; (3) Preparing a phase separation system: placing the phase separation liquid in a low-temperature cooling bath for precooling; the precooling temperature is -40°C to -20°C; the phase separation liquid is petroleum ether; (4) adding the w / o type emulsion to the precooled phase separation liquid and stirring until the phase separation is complete; the speed of adding the w / o type emulsion to the phase separation liquid is 1 to 2 mL / s, and the phase separation time is 30 to 40 min; After phase separation occurs, stirring and replacing the phase separation liquid to repeat this step; starting from the occurrence of phase separation, the phase separation liquid is replaced once every 10 minutes for 3 times; the stirring is magnetic stirring, and the speed of the magnetic stirring is 1000 or 1500 rpm; (5) After filtration, freeze-drying is performed to obtain microcarrier particles.

2. The method for preparing microcarriers for cell cultured meat production based on a novel low temperature induced phase separation technology according to claim 1, characterized in that: The mass volume ratio of the phase separation liquid to the w / o type emulsion is 4 / 1 to 5 / 1.

3. The method for preparing microcarriers for cell cultured meat production based on a novel low temperature induced phase separation technology according to claim 1, characterized in that: The mass fraction of the raw aqueous solution is 0.02-0.1; the mass volume ratio of the raw aqueous solution to the oil phase solvent is 0.5 / 1.

4. The method for preparing microcarriers for cell cultured meat production based on a novel low temperature induced phase separation technology according to claim 1, characterized in that: The mass volume ratio of the emulsifier to the oil phase solvent is 0.01 / 1 to 0.05 / 1; the mass fraction of the aqueous solution of the crosslinking agent is 0.05 to 0.1, and the mass volume ratio of the crosslinking agent aqueous solution to the oil phase solvent is 0.01 / 1 to 0.05 / 1.

Citation Information

Patent Citations

  • Cereal protein-based micro-carrier for large-scale culture of cells, and preparation method and application of micro-carrier

    CN102516778A

  • Composite microcarrier for manufacturing cell culture meat and preparation method of composite microcarrier

    CN113684177A

  • Edible microcarrier for cell meat and preparation method thereof

    CN116536257A

  • Low-cost edible microcarrier for cell culture meat production and preparation method thereof

    CN117701497A

  • Method for preparing hollow / open regenerated cellulose microspheres based on phase separation

    CN118325167A