High-toughness copolymer transparent polyamide and preparation method thereof

By introducing long-chain monomers with side group structures into the polyamide molecular chain, the problem of insufficient flexibility and processing performance of transparent nylon materials is solved, and a copolymerized transparent polyamide material with high toughness and high transparency is achieved, which is suitable for a wide range of industries. application.

CN118580488BActive Publication Date: 2024-10-29SHANDONG GUANGYIN NEW MATERIALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411073622.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-29
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The inherent amorphous or microcrystalline structure of transparent nylon materials results in low flexibility, insufficient fluidity during processing, and limited low-temperature resistance, which limits its promotion and application in wider industrial fields.

Method used

By introducing long-chain monomers with side group structures into the polyamide molecular chain and using a specific copolymerization process, high-toughness copolymerized transparent polyamide is prepared to ensure high transparency and excellent impact resistance of the material and avoid phase separation problems. .

Benefits of technology

It improves the toughness and processing performance of the material, maintains high transparency, extends the service life of the material, and improves the overall reliability and performance stability of the product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of polyamide, and specifically relates to high-toughness copolymer transparent polyamide and its preparation method. It is prepared by copolymerization reaction of polymerization monomers of alicyclic diamine, aliphatic dicarboxylic acid, aliphatic diamine with a side group structure and aliphatic dibasic acid with a side group structure under the action of a catalyst, and the molar percentages are as follows: alicyclic diamine: 37~45mol%; aliphatic dicarboxylic acid: 37~45mol%; aliphatic diamine with a side group structure: 5~13mol%; aliphatic dibasic acid with a side group structure: 5~13mol%; by introducing a long-chain monomer with a side group structure into the molecular chain, not only the toughness of the material is enhanced, its processing performance is optimized, but also the original high transparency of the material is ensured to be maintained. The obtained polyamide material exhibits good impact resistance and effectively avoids the problem of phase separation, thereby ensuring long-term stability during use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyamides, and in particular relates to high-toughness copolymer transparent polyamide and a preparation method thereof. Background Art

[0002] Polyamide, commonly known as nylon, is a class of polymer compounds that characteristically contain amide groups (-CONH-) in their main molecular chains. Among them, transparent nylon, as a special member of the polyamide family, exhibits a unique amorphous or slightly crystalline molecular structure, which gives it excellent light transmittance, usually reaching or exceeding 90%. In addition to the remarkable characteristic of high transparency, transparent nylon also has excellent dimensional stability, low molding shrinkage, excellent wear resistance, and the ability to be easily blended with other polyamide materials to form high-performance alloys. These comprehensive properties not only support its application as a single material, but also promote the improvement of its performance through alloying modification technology, thereby greatly expanding its application potential in multiple high-end fields.

[0003] Specifically, transparent nylon has been widely used in the manufacture of optical instruments with strict requirements on optical properties, the processing of precision parts with high standards for dimensional accuracy and wear resistance, the food packaging industry involving food safety standards, and the production of high-end sports equipment that pursues both lightness, high strength and beauty. However, despite the excellent performance of transparent nylon in many aspects, its inherent amorphous or microcrystalline structure also brings challenges, such as relatively low flexibility, insufficient fluidity during processing, and limited low temperature resistance. These problems have, to a certain extent, restricted the further promotion and application of transparent nylon in a wider range of industrial fields.

[0004] Chinese patent CN105949762A discloses a toughened transparent nylon and its preparation method, which improves the toughness of transparent nylon by adding a toughening agent. The process is simple, but it is subject to process conditions such as dispersion degree and compatibility, and is prone to poor compatibility with the blend or phase separation. It is not suitable for long-term use. In addition, the introduction of a toughening agent may also lead to a problem of reduced transparency. Therefore, a new copolymerization process is developed for the preparation of high-toughness transparent nylon resin, which gives the material the characteristics of high toughness while ensuring transparency, and has certain positive significance for the promotion of high-performance transparent nylon materials. Summary of the invention

[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a high-toughness copolymer transparent polyamide, which not only enhances the toughness of the material and optimizes its processing performance, but also ensures that the original high transparency of the material is maintained by introducing a long-chain monomer with a side group structure into the molecular chain;

[0006] Another object of the present invention is to provide a method for preparing a high-toughness copolymer transparent polyamide, which has a simple process and is easy to mass-produce. The obtained polyamide material exhibits good impact resistance and effectively avoids the phase separation problem that may be caused by the traditional blending process, thereby ensuring the long-term stability and excellent quality of the material during use.

[0007] The technical solution adopted by the present invention is as follows:

[0008] The high-toughness copolymer transparent polyamide is prepared by copolymerization of polymer monomers alicyclic diamine, aliphatic dicarboxylic acid, aliphatic diamine with a side group structure and aliphatic dibasic acid with a side group structure under the action of a catalyst, and the molar percentages thereof are respectively:

[0009] Alicyclic diamine: 37~45mol%

[0010] Aliphatic dicarboxylic acid: 37~45mol%

[0011] Aliphatic diamine with side group structure: 5~13mol%;

[0012] Aliphatic dibasic acid with side group structure: 5~13mol%;

[0013] The sum of alicyclic diamine, aliphatic dicarboxylic acid, aliphatic diamine with a side group structure and aliphatic dibasic acid with a side group structure is 100 mol%;

[0014] The amount of the catalyst used is 0.01-0.1wt.% of the total amount of the polymerization monomers;

[0015] The high-toughness copolymer transparent polyamide also includes an antioxidant, and the amount of the antioxidant is 0.1-0.5wt.% of the total amount of the polymerized monomers.

[0016] The alicyclic diamine is one of 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4-diaminodicyclohexylmethane or 4,4'-isopropyldicyclohexylamine.

[0017] The aliphatic dicarboxylic acid is one of sebacic acid, dodecanedioic acid or tetradecanedioic acid.

[0018] The aliphatic diamine with a side group structure is one of 2,2,4-trimethyl-1,6-hexanediamine, 5-methyl-1,9-nonanediamine or 2,4-dimethyl-1,8-octanediamine.

[0019] The aliphatic dibasic acid with a side group structure is 2-methyloctanedioic acid or 2,2,8,8-tetramethylazelaic acid.

[0020] The catalyst is one of sodium hypophosphite, hypophosphorous acid or potassium hypophosphite.

[0021] The antioxidant is one or more of antioxidant 1098, antioxidant 1010 or antioxidant 168.

[0022] The method for preparing the high-toughness copolymer transparent polyamide comprises the following steps:

[0023] (1) adding an alicyclic diamine, an aliphatic dicarboxylic acid, an aliphatic diamine with a side group structure, and an aliphatic dibasic acid monomer with a side group structure into deionized water, stirring at 50-100° C. to form a salt, thereby obtaining a salt solution;

[0024] (2) Add the salt solution to the reactor, then add the antioxidant and the catalyst, replace the nitrogen, evacuate the air in the reactor, and then heat the reactor. When the temperature in the reactor rises to a level where the stirrer can rotate, start stirring. When the temperature is further raised to 210-240°C, pressurize until the pressure reaches 0.5-3MPa, open the exhaust valve, maintain the pressure for 0.5-3h, slowly release the pressure for 0.5-3h to release water vapor. After the pressure is released, raise the temperature to 260-275°C, and carry out polymerization reaction at normal pressure for 0.5-2h. After the reaction is completed, open the bottom valve of the reactor, allow the polymer melt to pass through the cooling water tank for cooling, and obtain high-toughness copolymer transparent polyamide after pelletizing.

[0025] In the step (1), the mass ratio of the amount of deionized water added to the total amount of polymerization monomers is (1-1.2):1.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The high-toughness copolymer transparent polyamide described in the present invention not only enhances the toughness characteristics of the polyamide, but also improves its processing and molding performance by introducing a long-chain monomer with a side group structure into the polyamide molecular chain, thereby achieving a comprehensive improvement in material performance while ensuring that the transparency of the polyamide material is not affected;

[0028] (2) The high-toughness copolymer transparent polyamide described in the present invention has excellent impact resistance. At the same time, its unique molecular structure design effectively avoids the common phase separation phenomenon in the traditional blending process, thereby ensuring the performance stability of the material and the continuous consistency of product quality during long-term service. It not only extends the service life of the material, but also improves the overall reliability of the product;

[0029] (3) The method for preparing the high-toughness copolymer transparent polyamide of the present invention has a simple process, is easy to control, is convenient to operate, and is suitable for large-scale industrial production. DETAILED DESCRIPTION

[0030] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.

[0031] The raw materials used in the examples and comparative examples are conventional commercially available raw materials unless otherwise specified, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.

[0032] Example 1

[0033] The preparation method of the high-toughness copolymer transparent polyamide comprises the following steps:

[0034] (1) adding 3.155 kg (15 mol) of 4,4'-diaminodicyclohexylmethane, 3.454 kg (15 mol) of dodecanedioic acid, 1.58 kg (5 mol) of 2,2,4-trimethyl-1,6-hexanediamine and 1.22 kg (5 mol) of 2,2,8,8-tetramethylnonanediacid to 10 kg of deionized water, stirring at 80° C. to form a salt solution;

[0035] (2) The salt solution was added to a 50L polymerization kettle, and then 9.409g of antioxidant 1098 and 0.9409g of sodium hypophosphite were added. The polymerization kettle was closed and nitrogen was used to replace the air in the reactor by multiple inflation and exhaust. The air in the reactor was emptied and then the polymerization kettle was heated. When the temperature in the polymerization kettle reached a point where the agitator could rotate, stirring was started. When the temperature was further increased to 225°C and the pressure was increased to 1.7MPa, the exhaust valve was opened and the pressure was maintained for 2h. The pressure was slowly released for 1.5h to release water vapor. After the pressure was released, the temperature was increased to 265°C and the polymerization reaction was carried out at normal pressure for 0.75h. The pressure in the polymerization kettle was then reduced to -0.09MPa by vacuuming and the reaction was continued for 0.5h. After the reaction was completed, the bottom valve of the polymerization kettle was opened and the polymer melt was cooled through a cooling water tank. After pelletizing, a high-toughness copolymer transparent polyamide was obtained.

[0036] Example 2

[0037] The preparation method of the high-toughness copolymer transparent polyamide comprises the following steps:

[0038] (1) 3.576 kg (15 mol) of 3,3'-dimethyl-4,4-diaminodicyclohexylmethane, 3.454 kg (15 mol) of dodecanedioic acid, 1.58 kg (5 mol) of 2,2,4-trimethyl-1,6-hexanediamine and 1.22 kg (5 mol) of 2,2,8,8-tetramethylnonanediacid were added to 9.83 kg of deionized water, and the mixture was stirred at 50° C. to obtain a salt solution;

[0039] (2) The salt solution was added to a 50L polymerization kettle, and then 49.15g of antioxidant 1098 and 9.83g of sodium hypophosphite were added. The polymerization kettle was closed and nitrogen was used to replace the nitrogen by multiple inflation and exhaust. The air in the reactor was emptied and then the polymerization kettle was heated. When the temperature in the polymerization kettle reached a point where the agitator could rotate, stirring was started. When the temperature was further increased to 225°C and the pressure was increased to 1.7MPa, the exhaust valve was opened and the pressure was maintained for 2h. The pressure was slowly released for 1.5h to release water vapor. After the pressure was released, the temperature was increased to 265°C and the polymerization reaction was carried out at normal pressure for 0.75h. Then, the pressure in the polymerization kettle was reduced to -0.09MPa by vacuuming and the reaction was continued for 0.5h. After the reaction was completed, the bottom valve of the polymerization kettle was opened and the polymer melt was cooled through a cooling water tank. After pelletizing, a high-toughness copolymer transparent polyamide was obtained.

[0040] Example 3

[0041] The preparation method of the high-toughness copolymer transparent polyamide comprises the following steps:

[0042] (1) 3.79 kg (18 mol) of 4,4'-diaminodicyclohexylmethane, 3.64 kg (18 mol) of sebacic acid, 344.64 g (2 mol) of 5-methyl-1,9-nonanediamine and 376.44 g (2 mol) of 2-methyloctanedioic acid were added to 9.78 kg of deionized water, and stirred at 100° C. to obtain a salt solution;

[0043] (2) The salt solution was added to a 50L polymerization kettle, and then 24.4g of antioxidant 1098, 8.15g of antioxidant 168 and 2.44g of hypophosphorous acid were added. The polymerization kettle was closed and nitrogen was used to replace the air in the reactor by multiple inflation and exhaust. The air in the reactor was emptied and then the polymerization kettle was heated. When the temperature in the polymerization kettle reached a point where the agitator could rotate, stirring was started. When the temperature was further increased to 225°C and the pressure was increased to 1.5MPa, the exhaust valve was opened and the pressure was maintained for 2h. The pressure was slowly released for 1.5h to release water vapor. After the pressure was released, the temperature was increased to 260°C and the polymerization reaction was carried out at normal pressure for 0.75h. The pressure in the polymerization kettle was then reduced to -0.09MPa by vacuuming and the reaction was continued for 0.5h. After the reaction was completed, the bottom valve of the polymerization kettle was opened and the polymer melt was cooled through a cooling water tank. After pelletizing, a high-toughness copolymer transparent polyamide was obtained.

[0044] Example 4

[0045] The preparation method of the high-toughness copolymer transparent polyamide comprises the following steps:

[0046] (1) 4.291 kg (18 mol) of 4,4'-isopropyldicyclohexylamine, 4.290 kg (18 mol) of tetradecanedioic acid, 344.64 g (2 mol) of 2,4-dimethyl-1,8-octanediamine and 376.44 g (2 mol) of 2-methyloctanedioic acid were added to 9.4 kg of deionized water, and stirred at 100° C. to obtain a salt solution;

[0047] (2) The salt solution was added to a 50L polymerization kettle, and then 9.4g of antioxidant 1010 and 0.94g of potassium hypophosphite were added. The polymerization kettle was closed and nitrogen was used to replace the nitrogen by multiple inflation and exhaust. The air in the reactor was emptied and then the polymerization kettle was heated. When the temperature in the polymerization kettle reached a point where the agitator could rotate, stirring was started. When the temperature was further increased to 225°C and the pressure was increased to 1.6MPa, the exhaust valve was opened and the pressure was maintained for 2h. The pressure was slowly released for 1.5h to release water vapor. After the pressure was released, the temperature was increased to 275°C and the polymerization reaction was carried out at normal pressure for 0.75h. Then, the pressure in the polymerization kettle was reduced to -0.09MPa by vacuuming and the reaction was continued for 0.5h. After the reaction was completed, the bottom valve of the polymerization kettle was opened and the polymer melt was cooled through a cooling water tank. After pelletizing, a high-toughness copolymer transparent polyamide was obtained.

[0048] Comparative Example 1

[0049] The difference from Example 1 is that 2,2,4-trimethyl-1,6-hexanediamine and 2,2,8,8-tetramethylazelaic acid are not added to the formula components, and the rest is the same as Example 1.

[0050] Comparative Example 2

[0051] The difference from Example 2 is that 2,2,4-trimethyl-1,6-hexanediamine and 2,2,8,8-tetramethylazelaic acid are not added to the formula components, and the rest is the same as Example 2.

[0052] Comparative Example 3

[0053] The difference from Example 3 is that 5-methyl-1,9-nonanediamine and 2-methyloctanedioic acid are not added to the formula components, and the rest is the same as Example 3.

[0054] Comparative Example 4

[0055] The difference from Example 4 is that 2,4-dimethyl-1,8-octanediamine and 2-methyloctanedioic acid are not added to the formula components, and the rest is the same as Example 4.

[0056] Comparative Example 5

[0057] The difference between Comparative Example 5 and Example 1 is that 1,6-hexanediamine and 1,8-nonanedioic acid are used in equal molar amounts in the formula components to replace 2,2,4-trimethyl-1,6-hexanediamine and 2,2,8,8-tetramethylnonanedioic acid, and the rest is the same as Example 1.

[0058] The performance tests were performed on the polyamides prepared in Examples 1 to 4 and Comparative Examples 1 to 5, respectively, and the test methods were as follows:

[0059] Melting range (℃): Tested in accordance with ISO 3146;

[0060] Simple supported beam notched impact strength (kJ / m 2 ): Tested according to ISO 179, the test temperature is 23℃;

[0061] Simple supported beam low temperature notched impact strength (kJ / m 2 ): Tested in accordance with ISO 179, the test temperature is -30℃.

[0062] Light transmittance (%): The polyamide sample was made into a disk with a diameter of 40 mm and a thickness of 2 mm, and the light transmittance of the sample was tested using a light transmittance tester.

[0063] The test results are shown in Table 1.

[0064] Table 1 Performance test results

[0065] project Melting Range Simple supported beam notched impact strength Simple supported beam low temperature notched impact strength Light transmittance Example 1 165~190 18 16 91 Example 2 170~195 16 14 91 Example 3 160~190 20 18 91 Example 4 170~190 20 18 91 Comparative Example 1 170~200 11 10 92 Comparative Example 2 180~210 9 8 93 Comparative Example 3 170~200 10 9 91 Comparative Example 4 180~210 10 9 90 Comparative Example 5 175~210 15 12 85

[0066] It can be seen from the test data in Table 1 that by introducing a long-chain monomer with a side group structure, the simple supported beam notched impact strength and the simple supported beam low temperature notched impact strength of the polyamides prepared in Examples 1 to 4 are improved compared with Comparative Examples 1 to 4, that is, the toughness is improved; at the same time, the melting range of the polyamides prepared in Examples 1 to 4 is reduced compared with Comparative Examples 1 to 4, which is beneficial to the processing of the material; in addition, compared with Example 1, Comparative Example 5 introduces a long-chain monomer without a side group, so the material is more likely to crystallize, so the transparency of the material in Comparative Example 5 is reduced. The polyamides prepared in Examples 1 to 4 show an amorphous structure because the introduced side groups and aliphatic rings hinder crystallization, so they can still maintain good transparency.

Claims

1. A high-toughness copolymer transparent polyamide, characterized in that: It is prepared by copolymerization of alicyclic diamine, aliphatic dicarboxylic acid, aliphatic diamine with a side group structure and aliphatic dibasic acid with a side group structure under the action of a catalyst, and the molar percentages are: Alicyclic diamine: 37~45mol%; Aliphatic dicarboxylic acid: 37~45mol% Aliphatic diamine with side group structure: 5~13mol%; Aliphatic dibasic acid with side group structure: 5~13mol%; The sum of alicyclic diamine, aliphatic dicarboxylic acid, aliphatic diamine with a side group structure and aliphatic dibasic acid with a side group structure is 100 mol%; The amount of the catalyst used is 0.01-0.1wt.% of the total amount of the polymerization monomers; The high-toughness copolymer transparent polyamide also includes an antioxidant, and the amount of the antioxidant is 0.1-0.5wt.% of the total amount of the polymerized monomers; The aliphatic diamine with a side group structure is one of 2,2,4-trimethyl-1,6-hexanediamine, 5-methyl-1,9-nonanediamine or 2,4-dimethyl-1,8-octanediamine; The aliphatic dibasic acid with a side group structure is 2-methyloctanedioic acid or 2,2,8,8-tetramethylazelaic acid.

2. The high-toughness copolymer transparent polyamide according to claim 1, characterized in that: The alicyclic diamine is one of 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4-diaminodicyclohexylmethane or 4,4'-isopropyldicyclohexylamine.

3. The high-toughness copolymer transparent polyamide according to claim 1, characterized in that: The aliphatic dicarboxylic acid is one of sebacic acid, dodecanedioic acid or tetradecanedioic acid.

4. The high-toughness copolymer transparent polyamide according to claim 1, characterized in that: The catalyst is one of sodium hypophosphite, hypophosphorous acid or potassium hypophosphite.

5. The high-toughness copolymer transparent polyamide according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1098, antioxidant 1010 or antioxidant 168.

6. A method for preparing the high-toughness copolymer transparent polyamide according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) adding an alicyclic diamine, an aliphatic dicarboxylic acid, an aliphatic diamine with a side group structure, and an aliphatic dibasic acid monomer with a side group structure into deionized water, stirring to form a salt, and obtaining a salt solution; (2) Add the salt solution into the reactor, then add the antioxidant and the catalyst, and carry out the polymerization reaction after nitrogen substitution. After the reaction is completed, a high-toughness copolymer transparent polyamide is obtained.

7. The method for preparing the high-toughness copolymer transparent polyamide according to claim 6, characterized in that: In the step (1), the mass ratio of the amount of deionized water added to the total amount of the polymerized monomers is (1-1.2):1; and the temperature for stirring the salt is 50-100°C.

8. The method for preparing the high-toughness copolymer transparent polyamide according to claim 6, characterized in that: In the step (2), the polymerization reaction temperature is 260-275°C and the pressure is normal pressure.

Citation Information

Patent Citations

  • Toughened transparent nylon and preparation method thereof

    CN105949762A

  • Transparent polyamide and synthetic method thereof

    CN103483581A

  • Aliphatic transparent polyamide preparation method and aliphatic transparent polyamide

    CN106916296A

  • Preparation method of high temperature-resistant transparent polyamide

    CN109265677A

  • Transparent copolyamides

    GB8629928D0