A kind of docking process of high temperature resistant material
By using thermoplastic polyimide TPI layer and high-temperature resistant layer in the tape splicing, the problem of weak traditional splices and material waste is solved, and higher connection firmness and smoothness are achieved. and aesthetics, improving work efficiency and coil safety.
Patent Information
- Application Number
- CN202411052351.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The traditional belt splicing technology has the problems that the splicing joint is not strong enough, has poor flatness and aesthetics, and is prone to material breakage and material waste, which increases material costs and reduces work efficiency.
The splicing structure uses high-temperature resistant materials, including a thermoplastic polyimide TPI layer and a high-temperature resistant layer. The splicing base material is bonded at high temperature through a thermocompression bonding process, and the tackiness characteristics of the TPI layer are used to improve the connection firmness and The flatness and toughness of the structure are ensured through the positioning layer.
It improves the firmness, smoothness and aesthetics of the connection, reduces material waste, improves work efficiency, and enhances the safety of the coiled material.
Smart Images

Figure CN118580781B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material strip splicing, and in particular to a splicing process for high temperature resistant materials. Background Art
[0002] When replacing a new roll of material, the traditional practice is to stick three or more small pieces of tape with a length of 3 to 4 cm and a width of 1 to 2 cm on the joint of the new roll of material, so that they are evenly distributed, and the new substrate and the old substrate are connected by the small pieces of tape. However, when the small pieces of tape are bonded to the material, the joint is likely to be not strong enough. In order to increase the firmness of the connection between the tape and the substrate, the tape and the substrate are bound with a stapler, but the flatness and aesthetics are poor; and when the new substrate and the old substrate are connected by tape, the material may break, and re-joining the material will increase the material cost and reduce work efficiency. Summary of the invention
[0003] To overcome the above disadvantages, one of the purposes of the present invention is to provide a joint structure of high temperature resistant materials, which can make the joint more firm, flat and beautiful, and this joint structure can increase the safety of the coiled material and save material loss.
[0004] In order to achieve the above purpose, the technical solution adopted by the present invention is: a docking structure of high temperature resistant materials, comprising:
[0005] Docking components, wherein two groups of the docking components are provided, the two groups of the docking components are respectively located on the upper surface and the lower surface of the docking substrate, and the two groups of the docking components are symmetrically arranged with the docking substrate as a symmetry plane;
[0006] The docking assembly comprises a high temperature resistant layer and a TPI layer. The material of the TPI layer is thermoplastic polyimide. The TPI layer is arranged close to the docking substrate. The TPI layer can bond the high temperature resistant layer and the docking material.
[0007] Thermoplastic polyimide TPI is a high-performance special engineering plastic developed on the basis of traditional thermosetting polyimide (PI). TPI contains imide groups in the main chain of macromolecules, belongs to a class of heterocyclic polymers, and is one of the organic polymer materials with the best comprehensive performance. It has the characteristics of corrosion resistance, fatigue resistance, damage resistance, impact resistance, low density, low noise, long service life, and excellent high and low temperature performance (no deformation at -269℃~280℃ for a long time). The thermal decomposition temperature of TPI can reach up to 600℃, which is one of the polymers with the highest thermal stability so far.
[0008] By setting the TPI layer and utilizing the property of TPI becoming sticky when exposed to high temperature, the high temperature resistant layer and the docking substrate are bonded to improve the connection firmness of the high temperature resistant layer and the docking substrate; by simultaneously pressing the upper and lower hot pressing plates, the TPI can be heated and evenly bonded to the substrate to be docked in about 0.4S, which can improve the efficiency of the docking work; by covering the TPI layer with a high temperature resistant layer, on the one hand, it can be ensured that the TPI is heated evenly and becomes sticky evenly, and on the other hand, the toughness of the docking structure can be improved to prevent the docking structure from breaking, which would increase the material cost and reduce the work efficiency due to the re-docking of materials.
[0009] Furthermore, the docking material is generally a composite layer, including a metal layer and a PI layer, the metal layer is metal copper or metal aluminum, and the material of the high temperature resistant layer is the same as the material of the metal layer, or it can be different, and this application does not limit it. For example, if the material of the metal layer in the docking substrate is metal copper, the material of the high temperature resistant layer can be metal copper, metal aluminum, or other materials.
[0010] Furthermore, the length and width of the high temperature resistant layer are respectively greater than the length and width of the TPI layer, ensuring that the high temperature resistant layer can fully cover the TPI layer and prevent the TPI layer from being exposed. During lamination, the upper hot pressing plate or the lower hot pressing plate is pasted.
[0011] Further, the length of the high temperature resistant layer is 80~100mm, and the length of the TPI layer is 75~95mm. Exemplarily, the length of the high temperature resistant layer is 80mm, 82mm, 84mm, 86mm, 88mm, 90mm, 92mm, 94mm, 96mm, 98mm, 100mm or a range consisting of any two thereof, and the length of the TPI layer is 75mm, 77mm, 80mm, 82mm, 84mm, 86mm, 88mm, 90mm, 92mm, 95mm or a range consisting of any two thereof.
[0012] Further, the width of the high temperature resistant layer is 510~530mm, and the width of the TPI layer is 500~520mm. Exemplarily, the width of the high temperature resistant layer is 510mm, 515mm, 520mm, 525mm, 530mm or a range consisting of any two thereof, and the width of the TPI layer is 500mm, 505mm, 510mm, 515mm, 520mm or a range consisting of any two thereof.
[0013] Furthermore, a first positioning layer is provided between the docking assembly and the docking substrate. By providing the first positioning layer between the docking assembly and the docking substrate, the relative positions of the docking assembly and the docking substrate are pre-fixed to ensure that the docking assembly is located on the upper and lower surfaces of the docking location.
[0014] Furthermore, a second positioning layer is provided between the high temperature resistant layer and the TPI layer. By providing the second positioning layer between the high temperature resistant layer and the TPI layer, the relative positions of the high temperature resistant layer and the TPI layer are pre-fixed to prevent the high temperature resistant layer and the TPI layer from being misaligned.
[0015] Furthermore, the positioning layer includes a first positioning layer and a second positioning layer, and the positioning layer is a PI heat-resistant double-sided tape, which can be used to adhere to the docking components and docking substrates located on its upper and lower surfaces to fix the positions of the docking components and the docking substrates. The double-sided tape can be used to adhere to the high-temperature resistant layer and the TPI layer located on its upper and lower surfaces to fix the relative positions of the high-temperature resistant layer and the TPI layer.
[0016] Furthermore, the positioning layer is arranged on the upper and lower sides of the TPI layer. The positioning layer can be a continuous layered structure, which is used to pre-fix the relative position between the TPI layer and the high temperature resistant layer and the docking substrate. The continuous layered structure has a good fixing effect. On the same side of the TPI layer, multiple positioning layers can also be arranged, and gaps are left between the multiple positioning layers, which can not only play a role in pre-fixing, but also save the material of the positioning layer. The specific shape and number of the positioning layer are not limited, and it can play a role in pre-fixing the TPI layer, the high temperature resistant layer and the docking substrate. However, a positioning layer needs to be arranged at the docking point of the new substrate and the old substrate, which can connect the new substrate and the old substrate at the same time and pre-fix the relative position of the new substrate and the old substrate.
[0017] Another object of the present invention is to disclose a high-temperature material docking process, in which the docking substrates are docked using the docking structure as described above.
[0018] Furthermore, the high temperature material connection process comprises the following steps:
[0019] S1. Align the end of the new substrate with the end of the old substrate; specifically, overlap the new substrate with the old substrate, and then cut with a cutter to obtain a neat cut. Since the new substrate and the old substrate are cut by overlapping a portion, there is no restriction on the cutting direction of the cutter, and the ends of the new substrate and the old substrate must be aligned after cutting.
[0020] S2. Paste the docking structure at the docking point of the new substrate and the old substrate; specifically: turn the cut edges of the new substrate and the old substrate outward, and place the TPI layer with the positioning layer and the high-temperature resistant layer (docking structure) in the center just below the substrate to be docked; flatten the turned-out substrate inward and pre-press it onto the docking structure; prepare another docking mechanism, align its center position with the docking point, and pre-press it downward on the substrate.
[0021] S3. The joint mechanism is pressed by a hot pressing process to connect the new substrate and the old substrate at the joint.
[0022] Furthermore, in S3, in the hot pressing process, the docking mechanism is pressed by the upper heating pressing plate and the lower heating pressing plate, the hot pressing temperature is 380~400℃, and the hot pressing time is 0.4~120 seconds. The hot pressing pressure is 600~800kg. Since the docking structure is connected to the substrate by high-temperature pressing, the present application is suitable for the docking treatment of high-temperature resistant materials. The high temperature in the present application is a temperature greater than 400℃, and the high-temperature resistant material is a material whose properties will not change under a high-temperature environment of 400℃.
[0023] Further, in S3, at least two pressing protrusions are provided on the upper heating pressing plate and / or the lower heating pressing plate, and the pressing protrusions are symmetrically arranged on both sides of the docking point, and the pressing protrusions and the upper heating pressing plate or the lower heating pressing plate are close to each other to press the docking mechanism and the docking substrate.
[0024] Further, the length of the upper surface of the pressed protrusion is 15-25 mm, and the distance between the two pressed protrusions is 50-70 mm. The upper surface here refers to the surface close to the docking substrate. Exemplarily, the length of the upper surface of the pressed protrusion is 15 mm, 16 mm, 18 mm, 20 mm, 2 mm, 24 mm, 25 mm or a range consisting of any two thereof, and the distance between the two pressed protrusions is 50 mm, 53 mm, 55 mm, 58 mm, 60 mm, 63 mm, 65 mm, 68 mm, 70 mm or a range consisting of any two thereof.
[0025] Further, the length of the upper heating pressing plate or the lower heating pressing plate is 100-120 mm. Exemplarily, the length of the upper heating pressing plate or the lower heating pressing plate is 100 mm, 102 mm, 104 mm, 106 mm, 108 mm, 110 mm, 112 mm, 114 mm, 116 mm, 118 mm, 120 mm or a range consisting of any two thereof.
[0026] The beneficial effects of the present invention are:
[0027] 1) By setting the TPI layer and utilizing the property that TPI becomes sticky when exposed to high temperature, the high temperature resistant layer and the docking substrate are bonded to improve the connection firmness between the high temperature resistant layer and the docking substrate;
[0028] 2) By pressing the upper and lower hot pressing plates together at the same time, the TPI can be heated and evenly bonded to the substrate to be spliced in about 0.4 seconds, which can improve the efficiency of splicing work;
[0029] 3) By covering the TPI layer with a high temperature resistant layer, on the one hand, it can ensure that the TPI is heated evenly and becomes sticky evenly, and on the other hand, it can improve the toughness of the docking structure and prevent the docking structure from breaking, which will increase the material cost and reduce the work efficiency due to the re-docking of materials;
[0030] 4) Through the provision of multiple pressing protrusions, the joint mechanism and the new substrate and the old substrate can be pressed and connected, which ensures the firmness of the joint after pressing and also ensures the flatness of the joint after pressing. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 This is a schematic diagram of the superposition and cutting of the new substrate and the old substrate of the present invention;
[0034] Figure 2 This is a schematic diagram of the alignment of the new substrate and the old substrate after cutting according to the present invention;
[0035] Figure 3 It is a schematic diagram of the process of placing the docking mechanism on the lower surface of the docking position of the present invention;
[0036] Figure 4 This is a schematic diagram of the state in which the docking mechanism is placed on the lower surface of the docking position of the present invention;
[0037] Figure 5 It is a schematic diagram of the process of placing a docking mechanism on the upper surface of the docking position of the present invention;
[0038] Figure 6 This is a schematic diagram of the state in which the docking mechanism is placed on the upper surface of the docking position of the present invention;
[0039] Figure 7 It is a schematic diagram of the pressing process of the present invention;
[0040] Figure 8 This is a rendering of the upper surface of the substrate after lamination according to the present invention;
[0041] Fig. 9 This is a rendering of the lower surface of the substrate after lamination according to the present invention.
[0042] Among them: 1. docking substrate; 11. old substrate; 12. new substrate; 2. cutter; 3. docking assembly; 31. high temperature resistant layer; 32. TPI layer; 33. first positioning layer; 34. second positioning layer; 4. upper heating pressing plate; 5. lower heating pressing plate; 51. pressing protrusion. DETAILED DESCRIPTION
[0043] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0044] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0045] In the conventional splicing process, the new substrate 12 and the old substrate 11 are connected by adhesive tape, which easily makes the splicing part not firm enough, and has poor flatness and aesthetics.
[0046] See attached Figure 7 As shown, the present application provides a docking structure of a high temperature resistant material, including a docking assembly 3, wherein the docking assembly 3 is provided in two groups, and the two groups of the docking assembly 3 are respectively located on the upper surface and the lower surface of the docking substrate 1, and the two groups of the docking assembly 3 are symmetrically arranged with the docking substrate 1 as a symmetry plane. The docking substrate 1 includes a new substrate 12 and an old substrate 11, and the connection between the new substrate 12 and the old substrate 11 is a docking point. When the docking structure is arranged on the upper and lower surfaces of the docking substrate 1, the center position of the docking mechanism is aligned with the docking point, so that the docking structure is symmetrically arranged on the new substrate 12 and the old substrate 11.
[0047] In some embodiments, the docking assembly 3 includes a high temperature resistant layer 31 and a TPI layer 32 , wherein the TPI layer 32 is disposed close to the docking substrate 1 , and the TPI layer 32 can adhere to the high temperature resistant layer 31 and the docking substrate 1 .
[0048] The material of the TPI layer 32 is thermoplastic polyimide, and the melting point of the TPI material is between 350°C and 380°C. Through the TPI layer 32, during the high-temperature pressing process, the TPI material melts and bonds the high-temperature resistant layer 31 located on the upper and lower sides of the TPI layer 32 to the docking substrate 1. The upper and lower hot pressing plates are pressed at the same time, and the TPI can be heated and evenly bonded to the substrate to be docked in about 0.4S, which can improve the efficiency of docking work.
[0049] By setting the TPI layer 32 and the high temperature resistant layer 31, a good docking can be performed at a temperature of 400°C. TPI is an ultra-high temperature adhesive material that can bond the high temperature resistant layer 31 and the docking substrate 1 to make the docking more firm. And by bonding through the lamination process, the docking can be made smoother and more beautiful. Due to the high temperature resistant layer 31, it can be ensured that the TPI is heated evenly and can become sticky evenly, and the toughness of the docking structure can be improved to prevent the docking structure from breaking, which will increase the material cost and reduce the work efficiency due to the re-docking material.
[0050] In some embodiments, the docking component 3 also includes a positioning layer, which includes a first positioning layer 33 and a second positioning layer 34. The first positioning layer 33 is arranged between the TPI layer 32 and the docking substrate 1. By arranging the first positioning layer 33 between the TPI layer 32 and the docking substrate 1, the relative position of the docking component 3 and the docking substrate 1 is fixed to ensure that the docking component 3 is located on the upper and lower surfaces of the docking point, and the center position of the docking component 3 can face the docking point.
[0051] In some embodiments, a second positioning layer 34 is disposed between the high temperature resistant layer 31 and the TPI layer 32. By disposing the second positioning layer 34 between the high temperature resistant layer 31 and the TPI layer 32, the relative positions of the high temperature resistant layer 31 and the TPI layer 32 are fixed to prevent the high temperature resistant layer 31 and the TPI layer 32 from being misaligned.
[0052] In some embodiments, the first positioning layer 33 is a PI heat-resistant double-sided tape. The double-sided tape (first positioning layer 33) can adhere the docking component 3 and the docking substrate 1 located on its upper and lower surfaces. Before implementing the hot pressing process, the fixed docking component 3 and the docking substrate 1 are pre-bonded together, and then the relative position of the fixed docking component 3 and the docking substrate 1 is positioned by the first positioning layer 33 to prevent the relative position of the fixed docking component 3 and the docking substrate 1 from shifting.
[0053] In some embodiments, the second positioning layer 34 is also a PI heat-resistant double-sided tape. The double-sided tape (second positioning layer 34) can adhere the high temperature resistant layer 31 and the TPI layer 32 located on its upper and lower surfaces. Before implementing the hot pressing process, the high temperature resistant layer 31 and the TPI layer 32 are pre-bonded together, and then the relative position of the high temperature resistant layer 31 and the TPI layer 32 is positioned by the second positioning layer 34 to prevent the relative position of the high temperature resistant layer 31 and the TPI layer 32 from shifting.
[0054] In some embodiments, the length and width of the high temperature resistant layer 31 are respectively greater than the length and width of the TPI layer 32, ensuring that the high temperature resistant layer 31 can fully cover the TPI layer 32 to prevent the TPI layer 32 from being exposed. During lamination, the TPI material is adhered to the upper hot pressing plate or the lower hot pressing plate.
[0055] In some embodiments, the length of the high temperature resistant layer is 80-100 mm, the length of the TPI layer is 75-95 mm, the width of the high temperature resistant layer is 510-530 mm, and the width of the TPI layer is 500-520 mm.
[0056] In some embodiments, the docking material 1 is generally a composite layer, including a metal layer and a PI layer, the metal layer is metal copper or metal aluminum, and the material of the high temperature resistant layer is the same as the material of the metal layer, or it can be different, and this application does not limit it. For example, if the material of the metal layer in the docking substrate 1 is metal copper, the material of the high temperature resistant layer can be metal copper, metal aluminum, or other materials.
[0057] A high temperature material docking process, using any of the above-mentioned docking structures to dock a docking substrate 1, specifically comprising the following steps:
[0058] S1. See Appendix Figure 1~2 As shown, the end of the new substrate 12 is aligned with the end of the old substrate 11; specifically, the new substrate 12 and the old substrate 11 overlap a portion, and then the overlapping portion is cut with the cutter 2 to obtain a neat cut. Since the cutter 2 cuts the overlapping portion of the new substrate 12 and the old substrate 11, there is no restriction on the cutting direction of the cutter 2, and the ends of the new substrate 12 and the old substrate 11 must be aligned after cutting.
[0059] S2. See Appendix Figures 3 to 6 As shown, the docking structure is pasted at the docking point of the new substrate 12 and the old substrate 11; the cut ends of the new substrate 12 and the old substrate 11 are turned outward, and the TPI layer 32 with double-sided tape and the high temperature resistant layer 31 (docking structure) are centered and placed directly below the substrate to be docked; the turned-over substrate is flattened inward and pre-pressed onto the docking structure; another docking mechanism is prepared, its center position is aligned with the docking point, and it is pre-pressed downward on the substrate.
[0060] S3. See Appendix Figure 7 As shown, the new substrate 12 and the old substrate 11 are connected at the connection point by pressing the connection mechanism through a hot pressing process.
[0061] In the hot pressing process, the docking structure is pressed by a pressing machine, the hot pressing temperature is 380-400°C, the hot pressing time is 0.4-120 seconds, and the hot pressing pressure is 600-800kg. Since the docking structure and the docking substrate are docked by high-temperature pressing, the present application is suitable for the docking treatment of high-temperature resistant materials, and the high temperature in the present application is a temperature greater than 400°C.
[0062] In some embodiments, the laminating machine includes an upper heated laminating plate 4 and a lower heated laminating plate 5. During the laminating process, the docking substrate 1 and the docking component 3 are positioned by the positioning layer and then placed between the upper heated laminating plate 4 and the lower heated laminating plate 5. The upper heated laminating plate 4 and the lower heated laminating plate 5 are brought close to each other to heat and extrude the docking substrate 1 and the docking component 3, thereby docking the new substrate 12 and the old substrate 11.
[0063] In some embodiments, the length of the upper hot pressing plate and the lower pressing plate are the same, ranging from 100 to 120 mm, and the length of the high temperature resistant layer 31 is smaller than that of the upper pressing plate to ensure the effect of heating and pressing, and the length of the high temperature resistant layer 31 is 80 to 100 mm; the length of the TPI layer 32 is smaller than that of the high temperature resistant layer 31 to ensure that the high temperature resistant layer 31 covers the TPI layer 32, and the length of the TPI layer 32 is 75 to 95 mm.
[0064] In some embodiments, two pressing protrusions 51 are provided on the lower heating pressing plate 5, and the pressing protrusions 51 are located on both sides of the docking place, and the pressing protrusions 51 are pressed with the upper heating pressing plate 4. By pressing the two pressing protrusions 51 with the upper heating pressing plate 4, the pressing area of the lower heating pressing plate 5 and the upper heating pressing plate 4 is reduced, that is, the pressing width of the docking mechanism is reduced. Due to the reduction of the pressing width, the bubbles in the docking mechanism and the docking material being pressed are easier to be discharged during the pressing process, so that the docking mechanism at the pressing place after pressing can be made more flat and free of bubbles (see the attached Figure 8 and attached Fig. 9 As shown). Compared with the traditional upper and lower heating plates (flat structure) for pressing, the pressing area is larger. During the pressing process, bubbles cannot be discharged in time, resulting in uneven pressing.
[0065] By providing the two pressing protrusions 51 , the docking mechanism and the new substrate 12 and the old substrate 11 can be pressed and connected, thereby ensuring the firmness and flatness of the docking place after pressing.
[0066] In some embodiments, there are multiple pressing protrusions 51, such as 3, 4, 5..., as long as the firmness and flatness of the joint can be guaranteed after pressing, this application does not limit it.
[0067] In some embodiments, the length L of the upper surface of the pressing protrusion 51 is 15~25mm, that is, the pressing length range of each protrusion and the upper pressure plate is 15~25mm. Experimental studies have shown that if the length of the upper surface of the pressing protrusion 51 is too short, it will affect the connection firmness between the docking mechanism and the substrate. If the length of the upper surface of the pressing protrusion 51 is too long, it will affect the flatness between the docking mechanism and the substrate. Therefore, it is best to control the length of the upper surface of each pressing protrusion 51 to 15~25mm.
[0068] In some embodiments, the distance between the two pressing protrusions 51 is 50-70 mm. Experimental studies have shown that the two pressing protrusions 51 have the best firmness when the distance between them is 50-70 mm.
[0069] In some embodiments, two pressing protrusions 51 are provided on the upper heating pressing plate 4, and the lower heating pressing plate 5 is a planar structure. During the pressing process, the pressing protrusions 51 and the lower heating pressing plate 5 press the docking mechanism.
[0070] In some embodiments, a pressing protrusion 51 is provided on both the upper heating pressing plate 4 and the lower heating pressing plate 5, and the positions of the pressing protrusion 51 of the upper heating pressing plate 4 and the pressing protrusion 51 of the lower heating pressing plate 5 are adapted to each other, and the docking mechanism is pressed by the pressing protrusion 51 of the upper heating pressing plate 4 and the pressing protrusion 51 of the lower heating pressing plate 5.
[0071] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A process for joining high temperature resistant materials, characterized in that: The following steps are involved: S1, aligning the end of the new substrate (12) with the end of the old substrate (11); S2, pasting a docking structure at the docking point of the new substrate (12) and the old substrate (11); the docking structure comprises: A docking assembly (3), wherein two groups of the docking assembly (3) are provided, and the two groups of the docking assembly (3) are respectively located on the upper surface and the lower surface of the docking substrate (1), and the two groups of the docking assembly (3) are symmetrically arranged with the docking substrate (1) as a symmetry plane; The docking assembly (3) comprises a high temperature resistant layer (31) and a TPI layer (32), wherein the material of the TPI layer is thermoplastic polyimide, the TPI layer (32) is arranged close to the docking substrate (1), and the TPI layer (32) can bond the high temperature resistant layer (31) and the docking substrate (1); The length and width of the high temperature resistant layer (31) are respectively greater than the length and width of the TPI layer (32); A first positioning layer (33) is provided between the docking assembly (3) and the docking substrate (1), and a second positioning layer (34) is provided between the high temperature resistant layer (31) and the TPI layer (32); S3, pressing the connection mechanism and the connection substrate (1) by a hot pressing process, and connecting the connection point of the new substrate (12) and the old substrate (11); In the hot pressing process, the docking mechanism is pressed by an upper heated pressing plate (4) and a lower heated pressing plate (5), the hot pressing temperature is 380-400° C., the hot pressing time is 0.4-120 seconds, and the hot pressing pressure is 600-800 kg; At least two pressing protrusions (51) are arranged on the upper heating pressing plate (4) and / or the lower heating pressing plate (5), and the pressing protrusions (51) are symmetrically arranged on both sides of the docking position, and the pressing protrusions (51) and the upper heating pressing plate (4) or the lower heating pressing plate (5) are close to each other to press the docking mechanism and the docking substrate (1); The length of the upper surface of the pressing protrusion (51) is 15-25 mm, and the distance between two adjacent pressing protrusions (51) is 50-70 mm.
2. The process for joining high temperature resistant materials according to claim 1, characterized in that: The length of the upper heating pressing plate (4) or the lower heating pressing plate (5) is 100-120 mm, the length of the high temperature resistant layer (31) is 80-100 mm, and the length of the TPI layer is 75-95 mm.