A sealing material for membrane electrode and single cell and a preparation method thereof
By using a multi-layer structure of hot-melt adhesive layer material in the fuel cell, the problems of uneven force and insufficient sealing of the membrane electrode are solved, the performance consistency and service life of the fuel cell are improved, and the production cost is reduced.
Patent Information
- Application Number
- CN202411055547.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The membrane electrodes in existing fuel cells are unevenly stressed during the assembly process, resulting in poor performance consistency and short service life. The conventional sealing structure is difficult to ensure the uniform state of the membrane electrodes, which increases maintenance costs.
Using a hot-melt adhesive layer composed of polyolefin resin, polybutadiene resin, tackifying resin, thermoplastic elastomer resin and curing agent, the membrane electrode and the bipolar plate are bonded and sealed through a multi-layer structure design, improving the Sealing and stress buffering.
It improves the bonding strength and sealing of the membrane electrode, simplifies the production process, reduces the cost, extends the service life of the fuel cell, and avoids the problem of precipitation after being soaked in acid solution.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cell production, and in particular to a sealing material for a membrane electrode and a single cell and a preparation method thereof. Background Art
[0002] A fuel cell is a power generation device that converts the chemical energy present in fuel and oxidant directly into electrical energy. Fuel cells have the advantages of zero emission, no vibration or noise, good load responsiveness, and high reliability. Fuel cells can generally be divided into alkaline fuel cells, phosphoric acid fuel cells, molten carbonate fuel cells, solid oxide fuel cells, and proton exchange membrane fuel cells. Among them, proton exchange membrane fuel cells have high energy conversion efficiency, can be quickly started at room temperature, have no electrolyzed water loss, and have a long life. They have developed rapidly in recent years and are receiving increasing attention.
[0003] The core components of proton exchange membrane fuel cells include the first catalyst layer of the fuel cell, the proton exchange membrane, the second catalyst layer, the upper frame, the lower frame and the gas diffusion layers on both sides. The fuel cell membrane electrode manufacturing process usually includes catalyst slurrying, catalyst layer coating, frame bonding, gas diffusion layer coating, and gas diffusion layer bonding; the proton exchange membrane is very sensitive to temperature and humidity and is easily deformed with changes in ambient temperature and humidity. In addition to increasing the membrane strength outside the effective area of the electrode to stabilize the size of the membrane electrode, the frame can also prevent the direct contact between the proton membrane and the plate from causing mechanical damage and affecting the service life of the entire fuel cell. Therefore, an effective sealing frame can greatly improve the operating reliability and life of the fuel cell.
[0004] In the prior art, the blank area and the two sides of a certain size around the catalyst layer are directly fitted with the upper frame and the lower frame respectively, and then glue is applied on the bipolar plate to bond and seal with the upper and lower frames. When assembling the stack, the carbon paper of the membrane electrode produces compression deformation, which will also cause uneven force on the single section of the membrane electrode in the stack, resulting in poor performance consistency and affecting the overall power generation performance of the stack; the uneven force on the single section of the membrane electrode is mostly caused by the thickness accuracy of the membrane electrode itself, the accuracy of the bipolar plate sealing line and the misalignment during the assembly process. During the long-term operation of the stack, the membrane electrode is under pressure for a long time, and in the conventional sealing structure, the sealing frame is much thinner than the carbon paper, so it is difficult to ensure that hundreds of membrane electrodes are in a good consistency state, which leads to overpressure or low performance of some membrane electrodes, causing abnormal maintenance of the stack, greatly increasing the operation and maintenance costs. When assembling the stack, the membrane electrode and the bipolar plate need to be accurately positioned so that the reaction gases on both sides of each layer of the membrane electrode can be accurately transferred to the designated area of the membrane electrode according to the flow channel on the bipolar plate, so as to achieve uniform power generation in each part. Summary of the invention
[0005] The first technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a sealing material for membrane electrode and single cell is provided to achieve bonding and sealing with bipolar plates and proton exchange membranes, effectively prevent damage to the carbon paper and catalyst layer due to excessive pressure in the battery stack, achieve effective support for the carbon paper, and ensure the consistency of the battery stack formed after stacking.
[0006] To solve the above-mentioned first technical problem, the technical solution of the present invention is:
[0007] A sealing material for a membrane electrode and a single cell, comprising a release layer I, a hot-melt adhesive layer I, a substrate layer, a hot-melt adhesive layer II and a release layer II which are sequentially laminated;
[0008] The hot melt adhesive layer I and the hot melt adhesive layer II are both composed of polyolefin resin, polybutadiene resin, tackifying resin, thermoplastic elastomer resin, curing agent, latent curing agent and diluting solvent.
[0009] Preferably, the weight ratio of the polyolefin resin, the polybutadiene resin, the tackifying resin, the thermoplastic elastomer resin, the curing agent, the latent curing agent and the dilution solvent is 100: (10-30): (10-30): (10-30): (10-30): (1-5): (0.5-2): (50-150).
[0010] Preferably, the release layer I and the release layer II are both grid release films or matte release films with a grid shape, and the thickness of the release layer I and the release layer II is 25-150 μm;
[0011] The substrate layer is one of PEN, PI, PPS, PEI, PSU, PPSU or PET materials, and the thickness of the substrate layer is 100-250 μm.
[0012] Preferably, the polyolefin resin is a non-chlorinated anhydride-modified polyolefin resin;
[0013] The molecular weight of the polyolefin resin is 10,000 to 50,000, and the acid value of the polyolefin resin is 2 to 50 mgKOH / g.
[0014] Preferably, the polybutadiene resin is a polybutadiene resin modified with a hydroxyl group, a carboxyl group or an epoxy group. The epoxy-modified polybutadiene resin is obtained by an oxidation reaction between a low molecular weight liquid polybutadiene resin and a peroxide diacid, and the reaction principle is as follows:
[0015]
[0016] Preferably, the tackifying resin is one of petroleum resin, terpene resin, and terpene phenolic resin;
[0017] The thermoplastic elastomer resin is an amino-terminated SEBS material.
[0018] Preferably, the curing agent is one of an epoxy curing agent, a non-blocked isocyanate curing agent, and a carbodiimide curing agent;
[0019] The latent curing agent is a blocked isocyanate curing agent, and the deblocking temperature of the blocked isocyanate curing agent is 110-130°C;
[0020] The thickness of the hot melt adhesive layer I and the hot melt adhesive layer II are both 25-80 μm.
[0021] Preferably, the dilution solvent is any one of ethyl acetate, acetone, butanone, cyclohexanone, methyl isobutyl ketone, toluene, xylene, and cyclohexane, or a mixed solution of two or more thereof.
[0022] The second technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a method for preparing a sealing material for a membrane electrode and a single cell is provided, wherein the prepared sealing material can not only effectively bond the membrane electrode and the bipolar plate but also has excellent sealing, low compression deformation and excellent stress buffering.
[0023] To solve the above second technical problem, the technical solution of the present invention is:
[0024] A method for preparing a sealing material for a membrane electrode and a single cell, comprising the following preparation steps:
[0025] S01. Preparation of polyolefin resin
[0026] Add polyolefin, toluene, acid anhydride and di-tert-butyl peroxide into the autoclave, heat while stirring, and react at 140-160° C. for 1-3 hours to obtain a reaction liquid;
[0027] The reaction solution is cooled to 40° C. to obtain a non-chlorinated acid anhydride-modified polyolefin resin;
[0028] S02. Preparation of hot melt adhesive
[0029] Adding polybutadiene resin, tackifying resin and thermoplastic elastomer resin to the non-chlorinated anhydride modified polyolefin resin solution prepared in S01, cooling to room temperature after complete dissolution and filtering, adding curing agent, latent curing agent and diluting solvent to the filtrate, stirring evenly and filtering through a 200-800 mesh filter or a 1-20 μm filter element to obtain a hot melt adhesive layer adhesive;
[0030] S03. Preparation of hot melt adhesive film for single cell
[0031] A hot melt adhesive layer is coated on one side of the substrate layer using a knife coater or a CED coater, and a release layer I is attached after drying to obtain a sealing material having a single-sided hot melt adhesive layer;
[0032] The other side of the substrate layer is coated with a hot melt adhesive layer using a knife coater or a CED coater, and after aging, a release layer II is attached to obtain a membrane electrode and a sealing material for a single cell having a double-sided hot melt adhesive layer.
[0033] Preferably, in step S01, the weight ratio of polyolefin, toluene, acid anhydride and di-tert-butyl peroxide is 100: (400-600): (15-25): (3-5).
[0034] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0035] 1. The present invention adopts a hot melt adhesive with excellent adhesion and hydrolysis resistance to prepare a sealing material product that can firmly bond the electrode plate and the proton exchange membrane. When preparing the membrane electrode, only one side needs to use this sealing material to bond the membrane electrode, which makes the production process of the membrane electrode with a single-frame structure simple and the efficiency and yield are significantly improved. Furthermore, when the single-frame membrane electrode material is used to make a single cell product, the process is simplified and the product consistency is improved, which not only reduces the cost of fuel cell single cell packaging but also improves production efficiency and yield.
[0036] 2. The present invention can not only firmly bond the bipolar plate materials but also support and seal the membrane electrode by coating hot-melt adhesive layers on both sides of materials such as PI, PEN, PPS, PPSU, PSU or PEI.
[0037] 3. The present invention avoids the precipitation problem of the sealing material after long-term immersion in acid solution by selecting materials without N, P, S and Al, Cu, Ni, Cd, Cr, Pb, and Fe to make the hot-melt adhesive layer, thereby greatly improving the service life of the membrane electrode.
[0038] 4. The present invention adopts PEN materials, PI materials, PPS materials, PEI materials or PPSU materials with excellent physical and mechanical properties, gas barrier properties, chemical stability, heat resistance, UV resistance, radiation resistance and other properties as the base material, and uses a hot melt adhesive with high bonding strength, low precipitates, low compression deformation and excellent aging resistance to simplify the packaging process of the membrane electrode and the production method of the single cell, thereby improving the service life of the single cell.
[0039] 5. The sealing material prepared by the present invention has the advantages of simple packaging process, low material cost and high durability in the single-frame structure single-cell design.
[0040] 6. The present invention mixes conventional curing agents and closed curing agents to ensure that the sealing materials for membrane electrodes and single cells have high bonding strength and sealing properties in the early stages of single cell production without any glue overflow problems. During use, the closed curing agent further reacts and cross-links due to high temperature, thereby avoiding the problem of insufficient sealing due to long-term compression and thinning of the glue overflow thickness under high temperature conditions. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the embodiments. Example 1
[0042] 1. Add 100g of propylene-1-butene copolymer (melting point 85°C), 400g of toluene, 15g of maleic anhydride, and 3g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 140°C for 3h. After cooling the obtained reaction solution to 40°C, 510g of non-chlorinated anhydride-modified polyolefin resin (acid value 12mgKOH / g, weight average molecular weight 45000, melting point 84°C) is obtained;
[0043] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 10g of Japan Tosoh epoxidized polybutadiene resin PB3600, 10g of Arizona terpene resin RE100L and 10g of Japan Asahi Kasei amino-terminated styrene block copolymer MPA10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot-melt adhesive layer adhesive;
[0044] 3. Add 1g of Japanese polyurethane isocyanate curing agent L-75, 1g of Lanxess blocked isocyanate curing agent BI7982 and 50g of toluene dilution solvent to the filtered hot-melt adhesive layer adhesive solution, stir evenly, and filter with a 400-mesh filter. Then, use a scraper coater to apply a 30μm hot-melt adhesive layer on one side of the 100μm PEN substrate layer. After drying, attach a 25μm release layer I and roll it up. Use a scraper coater or CED coater to apply a 30μm hot-melt adhesive layer on the other side of the substrate layer. After aging, attach a 25μm release layer II to obtain a membrane electrode and a sealing material for a single cell with a double-sided hot-melt adhesive layer. Example 2
[0045] 1. Add 100g of propylene-ethylene-1-butene copolymer (melting point 95°C), 500g of toluene, 20g of maleic anhydride, and 4g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 150°C for 2h. After cooling the obtained reaction solution to 40°C, 620g of non-chlorinated anhydride-modified polyolefin resin (acid value 19mgKOH / g, weight average molecular weight 48000, melting point 93°C) is obtained;
[0046] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 15g of Japan Tosoh epoxidized polybutadiene resin PB3600, 15g of Arizona terpene resin RE100L and 15g of Japan Asahi Kasei amino-terminated styrene block copolymer H1221 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0047] 3. Add 1.5g of Japanese polyurethane isocyanate curing agent L-75, 2g of Lanxess blocked isocyanate curing agent BI7982 and 100g of cyclohexane dilution solvent to the filtered hot melt adhesive solution, stir evenly, and filter with a 400-mesh filter. Then use a scraper coater to apply a 50μm hot melt adhesive layer on one side of the 100μm PPSU substrate layer. After complete drying, attach a 38μm release layer I and roll it up. Use a scraper coater or CED coater to apply a 50μm hot melt adhesive layer on the other side of the substrate layer. After aging, attach a 38μm release layer II to obtain a membrane electrode and a sealing material for a single cell with a double-sided hot melt adhesive layer. Example 3
[0048] 1. Add 100g of propylene-ethylene copolymer (melting point 85°C), 400g of toluene, 15g of maleic anhydride, and 3g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 150°C for 2h. After cooling the obtained reaction solution to 40°C, 505g of non-chlorinated anhydride-modified polyolefin resin (acid value 12mgKOH / g, weight average molecular weight 45000, melting point 84°C) is obtained;
[0049] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 20g of Japan Tosoh epoxidized polybutadiene resin PB3600, 10g of Arizona terpene resin NG98 and 13g of Japan Asahi Kasei amino-terminated styrene block copolymer MP10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0050] 3. Add 1.2g of Japanese polyurethane isocyanate curing agent L-75, 1g of Covestro blocked isocyanate curing agent BL3175 and 85g of butanone diluent solvent to the filtered hot melt adhesive solution, stir evenly, and filter with a 400-mesh filter. Then, use a scraper coater to apply a 50μm hot melt adhesive layer on one side of the 188μm PI substrate layer. After complete drying, attach a 50μm release layer I and roll it up. Use a scraper coater or CED coater to apply a 50μm hot melt adhesive layer adhesive on the other side of the substrate layer. After aging, attach a 50μm release layer II to obtain a membrane electrode and a sealing material for a single cell with a double-sided hot melt adhesive layer. Example 4
[0051] 1. Add 100g of propylene-ethylene copolymer (melting point 85°C), 600g of toluene, 15g of maleic anhydride, and 3g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 160°C for 1h. After cooling the obtained reaction solution to 40°C, 700g of non-chlorinated anhydride-modified polyolefin resin (acid value 12mgKOH / g, weight average molecular weight 45000, melting point 84°C) is obtained;
[0052] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 30g of Japan Tosoh epoxidized polybutadiene resin PB3600, 30g of Arizona terpene resin RE100L and 30g of Japan Asahi Kasei amino-terminated styrene block copolymer MP10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0053] 3. Add 5g of Starr carbodiimide curing agent XR-5580, 1g of Lanxess blocked isocyanate curing agent BI7982 and 100g of ethyl acetate diluent to the filtered hot melt adhesive solution, stir evenly and filter with a 400-mesh filter. Then, apply an 80μm hot melt adhesive layer on one side of the 100μm PEI substrate layer using a scraper coater. After drying, attach a 125μm release layer I and roll it up. Apply an 80μm hot melt adhesive layer adhesive on the other side of the substrate layer using a scraper coater or a CED coater. After aging, attach a 150μm release layer II to obtain a membrane electrode and a sealing material for a single cell with a double-sided hot melt adhesive layer. Example 5
[0054] 1. Add 100g of propylene-ethylene-1-butene copolymer (melting point 90°C), 480g of toluene, 25g of maleic anhydride, and 5g of di-tert-butyl peroxide into a 5L autoclave, heat while stirring, and react at 150°C for 2h. After cooling the obtained reaction solution to 40°C, 600g of non-chlorinated acid anhydride-modified polyolefin resin (acid value 23mgKOH / g, weight average molecular weight 47000, melting point 87°C) is obtained;
[0055] 2. Take 100g of the above non-chlorinated anhydride modified polyolefin resin and add it into the reactor, and continue to add 15g of Japan Tosoh epoxidized polybutadiene resin PB3600, 20g of Arizona terpene resin RE100L and 15g of Japan Asahi Kasei amino-terminated styrene block copolymer MP10 into the reactor in batches, and after complete dissolution, cool to room temperature, pour out and filter to obtain a hot melt adhesive;
[0056] 3. Add 3g Nan Ya epoxy resin NPES901, 0.5g Lanxess blocked isocyanate curing agent BI7982 and 150g mixed dilution solvent of cyclohexanone and xylene (volume ratio of cyclohexanone and xylene is 1:1) to the filtered hot melt adhesive solution, stir evenly and filter with a 400-mesh filter. Then, use a scraper coater to apply a 25μm hot melt adhesive layer on one side of the 130μm PET substrate layer. After drying, attach a 150μm release layer I and roll it up. Use a scraper coater or CED coater to apply a 25μm hot melt adhesive layer on the other side of the substrate layer. After aging, attach a 250μm release layer II to obtain a membrane electrode and a sealing material for a single cell with a double-sided hot melt adhesive layer. Comparative Example 1
[0057] The isocyanate curing agent L-75 produced by Japan Polyurethane was not added, and the rest was exactly the same as in Example 2. Comparative Example 2
[0058] The LANXESS blocked isocyanate curing agent BI7982 was not added, and the rest was exactly the same as in Example 2.
[0059] The performance of the membrane electrode and single cell sealing material products in the above-mentioned Examples 1-5 and Comparative Examples 1-2 were tested respectively. The specific test items and test methods are shown in Table 1, and the test results are shown in Table 2.
[0060] Table 1
[0061]
[0062] Table 2
[0063]
[0064] Among them: 1. The peel strength test adopts 140℃*60s*0.6Mpa hot pressing; 2. sf means that CCM has delamination phenomenon during the peel strength test.
[0065] It can be seen from the experimental data in the above table that a sealing material having excellent bonding strength to different pole plates and membrane electrodes and a low drop in peel strength after immersion in acid can be prepared by adding different proportions; at the same time, the sealing material prepared by the present invention has a small drop in peel strength after long-term immersion in acid and no precipitates affect the activity of the membrane electrode; the present invention uses anhydride-modified polyolefins in combination with polybutadiene resins with functional groups and SEBS thermoplastic elastomers with terminal amino groups to react and cross-link with curing agents to form an interpenetrating network structure, ensuring that there is no glue overflow during the initial hot pressing of the product, and the addition of latent curing agents can further cross-link to achieve the purpose of post-stage curing, thereby improving the temperature resistance and hydrolysis resistance of the hot-melt adhesive layer and reducing compression deformation.
[0066] It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.
Claims
1. A sealing material for a single cell, characterized in that: It includes a release layer I, a hot melt adhesive layer I, a substrate layer, a hot melt adhesive layer II and a release layer II which are sequentially laminated. The hot melt adhesive layer I and the hot melt adhesive layer II are both composed of polyolefin resin, polybutadiene resin, tackifying resin, thermoplastic elastomer resin, curing agent, latent curing agent and diluting solvent; The weight ratio of the polyolefin resin, the polybutadiene resin, the tackifying resin, the thermoplastic elastomer resin, the curing agent, the latent curing agent and the dilution solvent is 100: (10-30): (10-30): (10-30): (10-30): (1-5): (0.5-2): (50-150); The release layer I and the release layer II are both grid release films or matte release films with a grid shape, and the thickness of the release layer I and the release layer II is 25-150 μm; The substrate layer is one of PEN, PI, PPS, PEI, PSU or PET materials, and the thickness of the substrate layer is 100-250 μm; The polyolefin resin is a non-chlorinated anhydride-modified polyolefin resin; The molecular weight of the polyolefin resin is 10000 to 50000, and the acid value of the polyolefin resin is 2 to 50 mgKOH / g; The polybutadiene resin is a polybutadiene resin modified with a hydroxyl group, a carboxyl group or an epoxy group; The tackifying resin is one of petroleum resin, terpene resin and terpene phenolic resin; The thermoplastic elastomer resin is an amino-terminated SEBS material; The curing agent is one of an epoxy curing agent, a non-blocked isocyanate curing agent, and a carbodiimide curing agent; The latent curing agent is a blocked isocyanate curing agent, and the deblocking temperature of the blocked isocyanate curing agent is 110-130°C; The thickness of the hot melt adhesive layer I and the hot melt adhesive layer II are both 25-80 μm; The method for preparing the sealing material for a single cell comprises the following steps: S01. Preparation of polyolefin resin Add polyolefin, toluene, acid anhydride and di-tert-butyl peroxide into the autoclave, heat while stirring, and react at 140-160° C. for 1-3 hours to obtain a reaction liquid; The reaction solution is cooled to 40° C. to obtain a non-chlorinated acid anhydride-modified polyolefin resin; S02. Preparation of hot melt adhesive Adding polybutadiene resin, tackifying resin and thermoplastic elastomer resin to the non-chlorinated anhydride modified polyolefin resin solution prepared in S01, cooling to room temperature after complete dissolution and filtering, adding curing agent, latent curing agent and diluting solvent to the filtrate, stirring evenly and filtering through a 200-800 mesh filter or a 1-20 μm filter element to obtain a hot melt adhesive layer adhesive; S03. Preparation of hot melt adhesive film for single cell A hot melt adhesive layer is coated on one side of the substrate layer using a knife coater or a CED coater, and a release layer I is attached after drying to obtain a sealing material having a single-sided hot melt adhesive layer; The other side of the substrate layer is coated with a hot-melt adhesive layer adhesive using a knife coater or a CED coater, and after aging, a release layer II is attached to obtain a single cell sealing material with double-sided hot-melt adhesive layers.
2. A sealing material for a single cell as claimed in claim 1, characterized in that: The dilution solvent is any one of ethyl acetate, acetone, butanone, cyclohexanone, methyl isobutyl ketone, toluene, xylene, and cyclohexane, or a mixed solution of two or more thereof.
3. The sealing material for a single cell according to claim 1, wherein: In step S01, the weight ratio of polyolefin, toluene, acid anhydride and di-tert-butyl peroxide is 100: (400-600): (15-25): (3-5).
Citation Information
Patent Citations
Hot melt adhesive, hydrogen fuel cell packaging hot melt adhesive membrane based on hot melt adhesive and preparation method of hydrogen fuel cell packaging hot melt adhesive membrane
CN116656274A
Sealing material for single fuel cell and preparation method of sealing material
CN118165663A