A high-flexibility, high-strength titanium alloy foil and its preparation and application
Titanium alloy foil processed with specific ingredients and processes solves the problems of fatigue damage and insufficient strength of existing materials during high-frequency folding operations, achieving high strength, high flexibility and excellent fatigue resistance, and is suitable for 3C electronic products. The foldable screen meets the needs of long-term use and high performance.
Patent Information
- Application Number
- CN202411061687.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing materials used for folding screens of 3C electronic products, such as polyimide substrates, composite backsheets, hand-shredded steel, ultra-thin glass and plastic films, suffer from fatigue damage, insufficient strength, aging, brittleness, etc. during high-frequency folding operations. Problems such as flexibility conflicts make it difficult to meet long-term use and high-performance requirements.
Titanium alloy foils with specific composition ratios are used, including Ti, Nb, Zr, Sn and trace oxygen. Through vacuum induction melting, multiple forgings, triple rolling and heat treatment processes, high strength, high flexibility and excellent fatigue resistance are prepared. Titanium alloy foil, suitable for folding screens and related components of 3C electronic devices.
It achieves the performance of titanium alloy foils that are not damaged during high-frequency folding operations, provides significant strength and flexibility improvements, extends service life, reduces equipment weight, and improves overall performance stability.
Smart Images

Figure CN118581352B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of titanium alloys, and relates to a high-flexibility, high-strength titanium alloy foil and its preparation and application, and in particular to a high-strength, high-flexibility titanium alloy foil suitable for folding screen technology in 3C electronic products (computers, communications and consumer electronics). Background Art
[0002] The rapid development of consumer electronics products relies on flexible displays and corresponding supporting structures, in which the selection and performance of materials are crucial. At present, the main supporting materials used in the market include polyimide (PI) substrates, composite backplanes, hand-torn steel, and some ultra-thin glass and plastic films. However, these materials face many challenges in practical applications, the specific problems are as follows:
[0003] Polyimide (PI) substrate: (1) Fatigue failure: Although the PI substrate has good flexibility and heat resistance, the polymer molecular chain is prone to fatigue failure during repeated folding, causing the material to lose its original mechanical strength, develop microcracks, and ultimately fail; (2) Insufficient strength: Although the PI substrate has good flexibility, its strength is relatively low and it is difficult to provide sufficient support in large-screen devices, affecting the overall structural stability of the device; (3) Aging problem: The PI substrate is easily affected by environmental factors (such as temperature and humidity) during long-term use, causing aging, degradation of mechanical properties, and shortened lifespan.
[0004] Composite material backplane: (1) Interface damage: Composite materials are usually made of fiber-reinforced polymers. During multiple folding operations, micro cracks are easily generated at the interface between the fiber and the matrix, resulting in material delamination and peeling, and a decrease in overall strength. (2) Insufficient flexibility: Although the strength of composite materials is relatively high, their lack of flexibility makes it easy for stress concentration to occur in the folded state, leading to local damage. (3) Limited fatigue performance: Under high-frequency folding operations, the fatigue performance of composite materials is poor, and fatigue damage is prone to occur, which affects the service life.
[0005] Hand-tearable steel: Despite its high strength and durability, it is prone to fatigue cracks and microstructural changes during repeated folding, leading to material failure; its relatively large rigidity and high hardness make it easy to form stress concentration areas when folded, leading to local deformation or damage; in addition, hand-tearable steel is prone to scratches and wear during use, and corrodes under certain conditions, affecting long-term stability; its manufacturing process is complex and costly, and its performance may decline after processing, and its high density increases the weight of the equipment, which is not conducive to lightweight design. Therefore, it is necessary to overcome the problems of fatigue failure, insufficient flexibility, surface damage, processing difficulty and weight of hand-tearable steel to ensure its reliability and durability in practical applications.
[0006] Ultra-thin glass: (1) Brittleness problem: Although ultra-thin glass has good surface hardness and transparency, its brittleness problem is difficult to solve. It is easy to break when bent and folded and cannot withstand high-frequency folding operations; (2) Microcrack expansion: During multiple folding processes, microcracks are easily generated inside the glass material and gradually expand under the action of stress, eventually causing the material to break; (3) The contradiction between strength and flexibility: The high strength of ultra-thin glass cannot make up for its lack of flexibility, which limits its practical application.
[0007] Plastic film: (1) Insufficient strength and durability: such as PET film and TAC film, these materials have low mechanical strength and durability and cannot withstand high-frequency folding operations for a long time; (2) Permanent deformation: During repeated folding, plastic film is prone to permanent deformation, affecting the flatness and display effect of the screen; (3) Aging and embrittlement: Plastic film is easily affected by environmental factors during long-term use, causing aging and brittleness, resulting in a decrease in mechanical properties, and seriously affecting service life and reliability.
[0008] In order to make up for the shortcomings of existing materials when used in 3C electronic devices (including but not limited to screen back panels, folding screen hinges, screen cover panels, screen support layers and screen protective film structures, especially folding screens and other related components), the present invention provides a titanium alloy material with high strength, high flexibility and excellent fatigue resistance, which can withstand high-frequency folding operations and maintain its mechanical properties and reliability during long-term use. Summary of the invention
[0009] The present invention aims to provide a new high-performance titanium alloy foil and a preparation method thereof to solve the above-mentioned problems in the prior art. The titanium alloy foil provided by the present invention not only has high strength and high flexibility, but also has excellent fatigue resistance, can withstand continuous high-frequency folding operations without damage, and is suitable for folding screen mobile phones, tablet computers and other 3C electronic products.
[0010] To achieve the above object, the present invention adopts the following technical solutions:
[0011] The first aspect is a highly flexible and high-strength titanium alloy foil, the mass percentage of which satisfies the following: Ti: 57.5%~69.95%, Nb: 22%~26%, Zr: 2%~6%, Sn: 6%~10%, O: 0.05%~0.5%; the thickness is 0.01mm~0.20mm, the surface roughness Ra is 0.09~0.13, the tensile strength along any direction of the foil surface is 710MPa~1190MPa, the elastic modulus is 41GPa~69GPa, and the elastic strain is 1.1%~2.0%.
[0012] The second aspect of the present invention is to provide a method for preparing a high-strength and high-flexibility titanium alloy foil, which is carried out in the following steps:
[0013] Step 1: Raw material proportioning and preliminary smelting: Use sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide as raw materials for preliminary smelting, adjust the proportion of each component to form an alloy, and make the mass percentage of the element composition of the alloy meet the following requirements: Ti: 57.5%~69.95%, Nb: 22%~26%, Zr: 2%~6%, Sn: 6%~10%, O: 0.05%~0.5%;
[0014] Step 2: Alloy electrode preparation: After preliminary smelting, the alloy is pressed into alloy electrodes;
[0015] Step 3: Vacuum induction melting: Place the alloy electrode in a vacuum induction melting furnace and heat it in a vacuum degree of not less than 10 -5 Pa, the melting times are 2 to 4 times, and the alloy ingot is obtained;
[0016] Step 4: Forging and blanking: Heat the alloy ingot to 800℃~840℃, keep it warm for 60min, forge and blank with a deformation of 30%~35%, control the cooling rate to 20℃ / min to 25℃ / min after blanking, and cool it to room temperature;
[0017] Step 5: Forging treatment: heat the billeted alloy to 800℃~850℃, increase the temperature at a rate of 100℃ / min to 110℃ / min, keep warm for 60min, and the forging deformation is 50%~55%; among them, the forging passes are 3 times, and the cooling rate is controlled at 20℃ / min to 25℃ / min after forging, and then cool to room temperature;
[0018] Step 6: A room temperature aging treatment: Perform room temperature aging treatment for 3 to 7 days;
[0019] Step 7: Triple rolling: The forged alloy is triple rolled to obtain a slab;
[0020] Step 8: Cold rolling: cold rolling the slab obtained in step 7, with a deformation amount of 30% to 95%, controlling the final thickness, and obtaining a foil with a thickness of 0.01 mm to 0.2 mm;
[0021] Step 9: Rapid heating and cooling: Rapidly heat the foil to 800°C~880°C at a heating rate of 20°C / min to 100°C / min, keep warm for 10min to 20min, and then rapidly cool to room temperature at a cooling rate of 30°C / min to 50°C / min;
[0022] Step 10: Preliminary heat treatment: heat the cooled foil to 250-450°C at a rate of 100°C / min, keep it at that temperature for 1-20 minutes, then cool it at a rate of 10-25°C / min until the foil temperature is 100-120°C lower than the preliminary heat treatment temperature, keep it at that temperature for 10 minutes, and then air cool it to room temperature;
[0023] Step 11: Straightening treatment: The foil after the preliminary heat treatment is straightened at a temperature of 20°C to 500°C, a straightening force of 100kN to 500kN, and a strain of 0.01% to 0.30%;
[0024] Step 12: Secondary heat treatment: The straightened foil is subjected to secondary heat treatment, heating to 400-600°C at a rate of 100°C / min, keeping the temperature for 1-15min, then cooling at a rate of 30°C / min until the foil temperature is 100-250°C lower than the secondary heat treatment temperature, keeping the temperature for 1-30min, and then air cooling to room temperature;
[0025] Step 13: Secondary room temperature aging treatment: Perform room temperature aging treatment for 1 to 3 days to obtain a highly flexible and high-strength titanium alloy foil.
[0026] Among them, the triple rolling process is:
[0027] First heavy rolling: the material is heated to 300℃~900℃ and then kept warm for 30min~120min, and then the first heavy rolling is carried out with 3~4 passes. After rolling, it is cooled to 0~400℃ and kept warm with a cooling rate of 25~27℃ / min; among which, the deformation of the first heavy rolling is 10%~40%.
[0028] Second rolling: the material is heated to 300℃~700℃ and then kept warm for 30min~120min, then the direction is changed by 90° for the second rolling, with 4 passes. After rolling, it is cooled to room temperature with a cooling rate of 25~27℃ / min. Among them, based on the material obtained after the first rolling, the deformation of the second rolling is 10%~40%.
[0029] The third rolling: the material is heated to 20℃~400℃ and then kept warm for 30min~120min, then the direction is changed by 90° for the third rolling, the number of rolling passes is 3~5, and the material is cooled to room temperature after rolling, with a cooling rate of 25~27℃ / min; among them, based on the material obtained after the second rolling, the deformation of the third rolling is 10%~40%.
[0030] The third aspect of the present invention is the application of the high-flexibility, high-strength titanium alloy foil in 3C electronic devices, including but not limited to screen back panels, folding screen hinges, screen cover panels, screen support layers and screen protective film structures; wherein 3C electronic devices are computer, communication and consumer electronic devices.
[0031] The high-flexibility and high-strength titanium alloy foil provided in the present invention is prepared by improving the processing technology and has the following advantages:
[0032] 1. High strength: The strength of the titanium alloy foil provided by the present invention is 710MPa~1190MPa, which is significantly higher than traditional polymer, aluminum alloy, copper alloy and other foils, and can provide better support effect and ensure the structural stability of the folding screen.
[0033] 2. High flexibility: The elastic strain of the titanium alloy foil provided by the present invention is 1.1% to 2.0%, which is significantly higher than that of metal foils such as hand-torn steel, and can effectively prevent the material from bending and breaking.
[0034] 3. Lightweight: By adjusting the composition ratio, the density of the titanium alloy foil provided by the present invention is not higher than 6.0g / cm 3 , which helps reduce the overall weight of the device and improves portability.
[0035] The principle of the present invention is as follows:
[0036] 1. Composition design: The present invention regulates the mass percentage of titanium (Ti), niobium (Nb), zirconium (Zr), tin (Sn) and trace oxygen (O) through precise alloy composition design to ensure that the alloy has excellent comprehensive mechanical properties. Titanium, as a base metal, provides excellent specific strength and corrosion resistance. The introduction of niobium not only enhances the solid solution strengthening effect, but also improves the toughness and flexibility of the alloy by increasing the lattice distortion. The addition of zirconium refines the grain structure and improves the plasticity and fatigue resistance of the alloy. Tin improves the low-temperature toughness and creep resistance of the alloy. Trace amounts of oxygen further improve the strength of the alloy through solid solution strengthening. This composition design precisely regulates the proportion and distribution of each element at the atomic scale, giving full play to the synergistic strengthening effect of the multi-element alloy.
[0037] 2. Improved flexibility: The present invention adopts a series of advanced process technologies to improve the flexibility of the alloy. First, through vacuum induction melting under high vacuum conditions, the alloy composition is highly homogenized and impurities and defects are eliminated. Then, multiple high-temperature forging and blanking treatments are used to promote dynamic recrystallization and form a uniform and fine grain structure. In the triple rolling process, through multiple alternating rolling passes, an orderly grain orientation is generated, the texture structure is optimized, and the flexibility of the alloy is significantly improved. In the rapid heating and cooling stage, the heating and cooling rates are strictly controlled, and the dynamic adjustment effect of nano-scale composition inhomogeneity (Dynamic Adjustment of Nano-scale Composition Inhomogeneity, DANCII) is used to achieve the enhancement of grain boundaries and the entanglement of dislocations, further improving the flexibility of the alloy.
[0038] 3. Improve performance: Other public technical solutions in this field can provide plates with superelastic properties. However, the superelastic properties of alloys are closely related to the thickness of the product. When the thickness of the product is reduced from millimeter level to micrometer level using conventional processes, the performance of the material will change completely and the superelasticity will disappear. Therefore, although there are technical solutions for superelastic plates, it is impossible to inspire relevant technicians to obtain superelastic foils, and there is currently no technical solution for preparing superelastic and flexible foils. The present invention significantly improves the overall performance of the alloy through a multi-level heat treatment process. Specifically, during the initial heat treatment and secondary heat treatment, the uneven distribution of nanoscale components is optimized by precisely controlling the aging temperature and the holding time, forming a nanostructure with high density and high stability, and enhancing the strength and toughness of the alloy. Through room temperature aging treatment, the internal residual stress is released, the microstructure is stabilized, and the dimensional stability and fatigue performance of the material are improved. In the straightening stage, high-precision straightening equipment and precise mechanical parameter control are used to ensure the flatness and surface quality of the foil. The titanium alloy foil finally prepared has a thickness ranging from 0.01 mm to 0.20 mm, a surface roughness Ra of 0.09 to 0.13, a tensile strength of 710 MPa to 1190 MPa, an elastic modulus of 41 GPa to 69 GPa, and an elastic strain of 1.1% to 2.0%.
[0039] 4. Heat treatment process: The disclosed technology in the art generally adopts the solid solution and water quenching process when preparing foil, but the present invention does not adopt the traditional solid solution treatment and water quenching process. This is because the solid solution treatment and water quenching process easily introduce internal stress and microcracks, resulting in instability of material properties. By avoiding these processes, the present invention ensures that the internal structure of the material is more uniform, reduces the generation of defects, and thus improves the overall performance and service life of the alloy. In particular, in the optimization process of dynamic recrystallization and nanoscale component inhomogeneity, high-temperature solid solution treatment and drastic cooling are not required, and excellent mechanical properties and flexibility can still be achieved.
[0040] 5. Strict control of process sequence: The preparation method of the present invention must be carried out strictly in accordance with the given step sequence. Each process step is carried out on the basis of the previous step, ensuring the optimization of the microstructure and performance of the alloy at each stage. For example, the alloy electrode after the initial smelting needs to be smelted multiple times under high vacuum conditions to ensure the uniformity of the composition, and this uniformity is the basis for subsequent high-temperature forging and blanking treatment. For another example, in the triple rolling process, multiple passes of alternating rolling and insulation treatment at a specific temperature are all to optimize the grain structure and composition distribution at different scales and improve the comprehensive performance of the material. The strict process sequence not only ensures the effectiveness of each step, but also avoids mutual interference in the process, ensuring that the final prepared titanium alloy foil has stable and excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The present invention is a flow chart of a method for preparing a high-flexibility and high-strength titanium alloy foil. DETAILED DESCRIPTION
[0042] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme of the present invention will be clearly and completely described below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work should fall within the scope of protection of the present invention. Among them, the preparation method of the high-flexibility and high-strength titanium alloy foil provided by the present invention is as follows: Figure 1 shown.
[0043] Example 1
[0044] Use sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide as raw materials for preliminary smelting, and adjust the composition content to the alloy element composition of Ti: 69.95%, Zr: 2%, Nb: 22%, Sn: 6%, O: 0.05%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted twice to obtain an alloy ingot. The alloy ingot was heated to 800℃, kept warm for 60min, forged with a deformation of 30% and then cooled to room temperature at a cooling rate of 20℃ / min. The alloy after billeting was heated to 800℃, heated at a rate of 100℃ / min, kept warm for 60min and then forged for 3 times with a total deformation of 50%, and then cooled to room temperature at a rate of 20℃ / min. Aging treatment at room temperature was performed for 7 days. Then, three rolling processes were carried out: the first rolling process was heated to 300℃, kept warm for 30min, the rolling deformation was 10%, rolled for 3 times, cooled to 0℃, and the cooling rate was 25℃ / min; the second rolling process was heated to 300℃, kept warm for 30min, rolled at 90°, the deformation was 10%, rolled for 4 times, cooled to room temperature, and the cooling rate was 25℃ / min; the third rolling process was heated to 20℃, kept warm for 30min, rolled at 90° again, the deformation was 10%, rolled for 5 times, cooled to room temperature, and the cooling rate was 25℃ / min to obtain the slab. The slab was cold rolled with a deformation of 30% to obtain a foil with a thickness of 0.2mm. The foil was rapidly heated to 800℃, the heating rate was 20℃ / min, kept warm for 10min, and then rapidly cooled to room temperature, and the cooling rate was 30℃ / min. The cooled foil is heated to 250°C at a rate of 100°C / min, kept warm for 1 minute, cooled to 140°C and kept warm for 10 minutes, with a cooling rate of 10°C / min, and then air-cooled to room temperature. The foil is straightened at a straightening temperature of 20°C, a straightening force of 500kN, and a strain of 0.01%. The straightened foil is heated to 250°C at a rate of 100°C / min, kept warm for 1 minute, cooled to 140°C, and kept warm for 1 minute, with a cooling rate of 30°C / min, and then air-cooled to room temperature. Room temperature aging treatment is performed for 1 day. Finally, a highly flexible and high-strength titanium alloy foil is obtained. The obtained highly flexible and high-strength titanium alloy foil can be well used in folding screen hinges.
[0045] Example 2
[0046] Sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide are used as raw materials for preliminary smelting, and the component content is adjusted to the alloy element composition of Ti: 57.5%, Zr: 6%, Nb: 26%, Sn: 10%, O: 0.5%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrode is placed in a vacuum induction melting furnace and the vacuum degree is not less than 10 -5Pa was melted three times to obtain an alloy ingot. The alloy ingot was heated to 820℃, kept warm for 60min, forged with a deformation of 35% and then cooled to room temperature at a cooling rate of 25℃ / min. The alloy after billeting was heated to 850℃, heated at a rate of 110℃ / min, kept warm for 60min and then forged for 3 times with a total deformation of 55%, and then cooled to room temperature at a rate of 25℃ / min. Aging treatment at room temperature was performed for 7 days. Then, three rolling processes were carried out: the first rolling process was heated to 900℃, kept warm for 120min, the rolling deformation was 40%, rolled 4 times, cooled to 400℃, and the cooling rate was 25℃ / min; the second rolling process was heated to 700℃, kept warm for 120min, rolled at 90°, the deformation was 40%, rolled 4 times, cooled to room temperature, and the cooling rate was 25℃ / min; the third rolling process was heated to 400℃, kept warm for 120min, rolled at 90° again, the deformation was 40%, rolled 3 times, cooled to room temperature, and the cooling rate was 25℃ / min to obtain the slab. The slab was cold rolled with a deformation of 95% to obtain a foil with a thickness of 0.01mm. The foil was rapidly heated to 880℃, the heating rate was 100℃ / min, kept warm for 20min, and then rapidly cooled to room temperature, and the cooling rate was 50℃ / min. The cooled foil was heated to 450°C at a rate of 100°C / min, kept warm for 20 minutes, cooled to 340°C and kept warm for 10 minutes at a cooling rate of 25°C / min, and then air-cooled to room temperature. The foil was straightened at a straightening temperature of 500°C, a straightening force of 400kN, and a strain of 0.3%. The straightened foil was heated to 600°C at a rate of 100°C / min, kept warm for 15 minutes, cooled to 350°C and kept warm for 30 minutes at a cooling rate of 30°C / min, and then air-cooled to room temperature. A room temperature aging treatment was performed for 3 days. Finally, a highly flexible and high-strength titanium alloy foil was obtained. The obtained highly flexible and high-strength titanium alloy foil can be well used in screen backplanes.
[0047] Example 3
[0048] Use sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide as raw materials for preliminary smelting, and adjust the composition content to the alloy element composition of Ti: 65.8%, Zr: 3%, Nb: 23%, Sn: 8%, O: 0.2%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted twice to obtain an alloy ingot. The alloy ingot was heated to 830°C, kept warm for 60 minutes, forged with a deformation of 30%, and then cooled to room temperature at a cooling rate of 20°C / min. The alloy after billeting was heated to 810°C, heated at a rate of 100°C / min, and forged after keeping warm for 60 minutes. The forging was performed 3 times with a total deformation of 50%, and then cooled to room temperature at a rate of 20°C / min. Aging treatment at room temperature was performed for 3 days. Then, three rolling processes were carried out: the first rolling process was heated to 620℃, kept warm for 60min, the rolling deformation was 30%, rolled for 3 times, cooled to 220℃, and the cooling rate was 25℃ / min; the second rolling process was heated to 510℃, kept warm for 60min, rolled at 90°, the deformation was 30%, rolled for 4 times, cooled to room temperature, and the cooling rate was 25℃ / min; the third rolling process was heated to 310℃, kept warm for 60min, rolled at 90° again, the deformation was 30%, rolled for 3 times, cooled to room temperature, and the cooling rate was 25℃ / min to obtain the slab. The slab was cold rolled with a deformation of 50% to obtain a foil with a thickness of 0.1mm. The foil was rapidly heated to 870℃, the heating rate was 50℃ / min, kept warm for 15min, and then rapidly cooled to room temperature, and the cooling rate was 30℃ / min. The cooled foil was heated to 420°C at a rate of 100°C / min, kept warm for 20 minutes, cooled to 310°C and kept warm for 10 minutes, with a cooling rate of 20°C / min, and then air-cooled to room temperature. The foil was straightened at a straightening temperature of 230°C, a straightening force of 110kN, and a strain of 0.12%. The straightened foil was heated to 420°C at a rate of 100°C / min, kept warm for 15 minutes, cooled to 310°C and kept warm for 10 minutes, with a cooling rate of 30°C / min, and then air-cooled to room temperature. Room temperature aging treatment was performed for 2 days. Finally, a highly flexible and high-strength titanium alloy foil was obtained. The obtained highly flexible and high-strength titanium alloy foil can be well used in the protective layer of folding screens.
[0049] Example 4
[0050] Sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide are used as raw materials for preliminary smelting, and the component content is adjusted to the alloy element composition of Ti: 66.8%, Zr: 4%, Nb: 22%, Sn: 7%, O: 0.2%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted 5 times to obtain an alloy ingot. The alloy ingot was heated to 840℃, kept warm for 60min, forged with a deformation of 32% and then cooled to room temperature at a cooling rate of 22℃ / min. The alloy after billeting was heated to 820℃, heated at a rate of 105℃ / min, kept warm for 60min and then forged, forged 3 times, with a total deformation of 52%, and then cooled to room temperature at a rate of 22℃ / min. Aging treatment at room temperature was performed for 4 days. Then, three rolling processes were carried out: the first rolling process was heated to 630℃, kept warm for 60min, with a rolling deformation of 32%, rolled for 3 times, cooled to 230℃, and a cooling rate of 27℃ / min; the second rolling process was heated to 520℃, kept warm for 60min, rolled at 90°, with a deformation of 32%, rolled for 4 times, cooled to room temperature, and a cooling rate of 27℃ / min; the third rolling process was heated to 320℃, kept warm for 60min, rolled at 90° again, with a deformation of 32%, rolled for 3 times, cooled to room temperature, and a cooling rate of 27℃ / min to obtain a slab. The slab was cold rolled with a deformation of 52% to obtain a foil with a thickness of 0.12mm. The foil was rapidly heated to 880℃, with a heating rate of 52℃ / min, kept warm for 15min, and then rapidly cooled to room temperature, with a cooling rate of 32℃ / min. The cooled foil was heated to 430°C at a rate of 100°C / min, kept warm for 20 minutes, cooled to 320°C and kept warm for 10 minutes, with a cooling rate of 22°C / min, and then air-cooled to room temperature. The foil was straightened at a straightening temperature of 240°C, a straightening force of 115kN, and a strain of 0.13%. The straightened foil was heated to 430°C at a rate of 100°C / min, kept warm for 15 minutes, cooled to 320°C and kept warm for 10 minutes, with a cooling rate of 30°C / min, and then air-cooled to room temperature. Room temperature aging treatment was performed for 2 days. Finally, a highly flexible and high-strength titanium alloy foil was obtained. The obtained highly flexible and high-strength titanium alloy foil can be well used in the protective layer of folding screens.
[0051] Example 5
[0052] Sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide are used as raw materials for preliminary smelting, and the component content is adjusted to the alloy element composition of Ti: 63.5%, Zr: 5%, Nb: 24%, Sn: 7%, O: 0.5%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted twice to obtain an alloy ingot. The alloy ingot was heated to 810℃, kept warm for 60min, forged with a deformation of 30% and cooled to room temperature at a cooling rate of 20℃ / min. The alloy after billeting was heated to 800℃, heated at a rate of 100℃ / min, kept warm for 60min and forged for 3 times with a total deformation of 50%, and then cooled to room temperature at a rate of 20℃ / min. Aging treatment at room temperature was performed for 5 days. Then, three rolling processes were carried out: the first rolling process was heated to 600℃, kept warm for 60min, the rolling deformation was 30%, rolled for 3 times, cooled to 200℃, and the cooling rate was 25℃ / min; the second rolling process was heated to 500℃, kept warm for 60min, rolled at 90°, the deformation was 30%, rolled for 4 times, cooled to room temperature, and the cooling rate was 25℃ / min; the third rolling process was heated to 300℃, kept warm for 60min, rolled at 90° again, the deformation was 30%, rolled for 3 times, cooled to room temperature, and the cooling rate was 25℃ / min to obtain the slab. The slab was cold rolled with a deformation of 50% to obtain a foil with a thickness of 0.07mm. The foil was rapidly heated to 850℃, the heating rate was 50℃ / min, kept warm for 15min, and then rapidly cooled to room temperature, and the cooling rate was 30℃ / min. The cooled foil is heated to 400℃ at a rate of 100℃ / min, kept at this temperature for 20min, cooled to 290℃ and kept at this temperature for 10min, with a cooling rate of 20℃ / min, and then air-cooled to room temperature. The foil is straightened at a straightening temperature of 200℃, a straightening force of 100kN, and a strain of 0.1%. The straightened foil is heated to 400℃ at a rate of 100℃ / min, kept at this temperature for 15min, cooled to 290℃ and kept at this temperature for 10min, with a cooling rate of 30℃ / min, and then air-cooled to room temperature. A room temperature aging treatment is performed for 2 days. Finally, a highly flexible and high-strength titanium alloy foil is obtained. The obtained highly flexible and high-strength titanium alloy foil can be well used in screen cover plates.
[0053] Example 6
[0054] Sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide are used as raw materials for preliminary smelting, and the component content is adjusted to the alloy element composition of Ti: 64.92%, Zr: 4%, Nb: 23%, Sn: 8%, O: 0.08%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted three times to obtain an alloy ingot. The alloy ingot was heated to 810℃, kept warm for 60min, forged with a deformation of 30% and then cooled to room temperature at a cooling rate of 20℃ / min. The alloy after billeting was heated to 820℃, heated at a rate of 100℃ / min, kept warm for 60min and then forged for 3 times with a total deformation of 50%, and then cooled to room temperature at a rate of 20℃ / min. Aging treatment at room temperature was performed for 4 days. Then, three rolling processes were carried out: the first rolling process was heated to 600℃, kept warm for 60min, the rolling deformation was 30%, rolled for 3 times, cooled to 200℃, and the cooling rate was 25℃ / min; the second rolling process was heated to 500℃, kept warm for 60min, rolled at 90°, the deformation was 30%, rolled for 4 times, cooled to room temperature, and the cooling rate was 25℃ / min; the third rolling process was heated to 300℃, kept warm for 60min, rolled at 90° again, the deformation was 30%, rolled for 3 times, cooled to room temperature, and the cooling rate was 25℃ / min to obtain the slab. The slab was cold rolled with a deformation of 50% to obtain a foil with a thickness of 0.09mm. The foil was rapidly heated to 850℃, the heating rate was 50℃ / min, kept warm for 15min, and then rapidly cooled to room temperature, and the cooling rate was 30℃ / min. The cooled foil is heated to 400℃ at a rate of 100℃ / min, kept at this temperature for 20min, cooled to 290℃ and kept at this temperature for 10min, with a cooling rate of 20℃ / min, and then air-cooled to room temperature. The foil is straightened at a straightening temperature of 200℃, a straightening force of 100kN, and a strain of 0.1%. The straightened foil is heated to 400℃ at a rate of 100℃ / min, kept at this temperature for 15min, cooled to 290℃ and kept at this temperature for 10min, with a cooling rate of 30℃ / min, and then air-cooled to room temperature. A room temperature aging treatment is performed for 2 days. Finally, a highly flexible and high-strength titanium alloy foil is obtained. The obtained highly flexible and high-strength titanium alloy foil can be well used in screen cover plates.
[0055] Example 7
[0056] Use sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide as raw materials for preliminary smelting, and adjust the composition content to the alloy element composition of Ti: 62.7%, Zr: 5%, Nb: 25%, Sn: 7%, O: 0.3%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted 4 times to obtain an alloy ingot. The alloy ingot was heated to 800℃, kept warm for 60min, forged with a deformation of 30% and then cooled to room temperature at a cooling rate of 20℃ / min. The alloy after billeting was heated to 820℃, heated at a rate of 100℃ / min, kept warm for 60min and then forged for 3 times with a total deformation of 50%, and then cooled to room temperature at a rate of 20℃ / min. Aging treatment at room temperature was performed for 5 days. Then, three rolling processes were carried out: the first rolling process was heated to 600℃, kept warm for 60min, the rolling deformation was 30%, rolled for 3 times, cooled to 200℃, and the cooling rate was 25℃ / min; the second rolling process was heated to 500℃, kept warm for 60min, rolled at 90°, the deformation was 30%, rolled for 4 times, cooled to room temperature, and the cooling rate was 25℃ / min; the third rolling process was heated to 300℃, kept warm for 60min, rolled at 90° again, the deformation was 30%, rolled for 3 times, cooled to room temperature, and the cooling rate was 25℃ / min to obtain the slab. The slab was cold rolled with a deformation of 50% to obtain a foil with a thickness of 0.1mm. The foil was rapidly heated to 850℃, the heating rate was 50℃ / min, kept warm for 15min, and then rapidly cooled to room temperature, and the cooling rate was 30℃ / min. The cooled foil is heated to 400°C at a rate of 100°C / min, kept warm for 20 minutes, cooled to 300°C and kept warm for 10 minutes, with a cooling rate of 20°C / min, and then air-cooled to room temperature. The foil is straightened at a straightening temperature of 200°C, a straightening force of 100kN, and a strain of 0.1%. The straightened foil is heated to 500°C at a rate of 100°C / min, kept warm for 15 minutes, cooled to 300°C and kept warm for 10 minutes, with a cooling rate of 30°C / min, and then air-cooled to room temperature. Room temperature aging treatment is performed for 2 days. Finally, a highly flexible and high-strength titanium alloy foil is obtained. The obtained highly flexible and high-strength titanium alloy foil can be well used in the support layer of folding screens.
[0057] Example 8
[0058] Sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide are used as raw materials for preliminary smelting, and the component content is adjusted to the alloy element composition of Ti: 63.6%, Zr: 5%, Nb: 24%, Sn: 7%, O: 0.4%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted three times to obtain an alloy ingot. The alloy ingot was heated to 810℃, kept warm for 60min, forged with a deformation of 30% and then cooled to room temperature at a cooling rate of 20℃ / min. The alloy after billeting was heated to 800℃, heated at a rate of 100℃ / min, kept warm for 60min and then forged for 3 times with a total deformation of 50%, and then cooled to room temperature at a rate of 20℃ / min. Aging treatment at room temperature was performed for 5 days. Then, three rolling processes were carried out: the first rolling process was heated to 600℃, kept warm for 60min, the rolling deformation was 30%, rolled for 3 times, cooled to 200℃, and the cooling rate was 25℃ / min; the second rolling process was heated to 500℃, kept warm for 60min, rolled at 90°, the deformation was 30%, rolled for 4 times, cooled to room temperature, and the cooling rate was 25℃ / min; the third rolling process was heated to 300℃, kept warm for 60min, rolled at 90° again, the deformation was 30%, rolled for 3 times, cooled to room temperature, and the cooling rate was 25℃ / min to obtain the slab. The slab was cold rolled with a deformation of 50% to obtain a foil with a thickness of 0.06mm. The foil was rapidly heated to 850℃, the heating rate was 50℃ / min, kept warm for 15min, and then rapidly cooled to room temperature, and the cooling rate was 30℃ / min. The cooled foil is heated to 420°C at a rate of 100°C / min, kept at this temperature for 20 minutes, then cooled to 300°C and kept at this temperature for 10 minutes, with a cooling rate of 20°C / min, and then air-cooled to room temperature. The foil is straightened at a straightening temperature of 200°C, a straightening force of 100kN, and a strain of 0.1%. The straightened foil is heated to 450°C at a rate of 100°C / min, kept at this temperature for 15 minutes, then cooled to 300°C and kept at this temperature for 10 minutes, with a cooling rate of 30°C / min, and then air-cooled to room temperature. A room temperature aging treatment is performed for 2 days. Finally, a highly flexible and high-strength titanium alloy foil is obtained. The obtained highly flexible and high-strength titanium alloy foil can be well applied to the screen backplane structure.
[0059] Comparative Example 1
[0060] Use sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide as raw materials for preliminary smelting, and adjust the composition content to the alloy element composition of Ti: 73.6%, Zr: 1%, Nb: 20%, Sn: 5%, O: 0.4%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted twice to obtain an alloy ingot. The alloy ingot was heated to 800℃, kept warm for 60min, forged with a deformation of 30% and then cooled to room temperature at a cooling rate of 20℃ / min. The alloy after billeting was heated to 800℃, heated at a rate of 100℃ / min, kept warm for 60min and then forged for 3 times with a total deformation of 50%, and then cooled to room temperature at a rate of 20℃ / min. Then, three rolling processes were carried out: the first rolling process was heated to 600℃, kept warm for 60min, the rolling deformation was 30%, rolled for 3 times, cooled to 200℃, and the cooling rate was 25℃ / min; the second rolling process was heated to 500℃, kept warm for 60min, rolled at 90°, the deformation was 30%, rolled for 4 times, cooled to room temperature, and the cooling rate was 25℃ / min; the third rolling process was heated to 300℃, kept warm for 60min, rolled at 90° again, the deformation was 30%, rolled for 3 times, cooled to room temperature, and the cooling rate was 25℃ / min to obtain the slab. The slab was cold rolled with a deformation of 50% to obtain a foil with a thickness of 0.15mm. The foil was rapidly heated to 850℃, the heating rate was 50℃ / min, kept warm for 15min, and then rapidly cooled to room temperature, and the cooling rate was 30℃ / min. The cooled foil was heated to 400°C at a rate of 100°C / min, kept at this temperature for 20 minutes, then cooled to 300°C and kept at this temperature for 10 minutes, with a cooling rate of 20°C / min, and then air-cooled to room temperature. The foil was straightened at a straightening temperature of 200°C, a straightening force of 100kN, and a strain of 0.1%. The straightened foil was heated to 400°C at a rate of 100°C / min, kept at this temperature for 15 minutes, then cooled to 300°C and kept at this temperature for 10 minutes, with a cooling rate of 30°C / min, and then air-cooled to room temperature. A room temperature aging treatment was performed for 2 days. Finally, a titanium alloy foil was obtained, but its composition did not meet the requirements, resulting in performance that did not meet expectations.
[0061] Comparative Example 2
[0062] Sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide are used as raw materials for preliminary smelting, and the component content is adjusted to the alloy element composition of Ti: 63.5%, Zr: 5%, Nb: 24%, Sn: 7%, O: 0.5%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted twice to obtain an alloy ingot. The alloy ingot was heated to 700℃, kept warm for 30min, forged with a deformation of 10% and then cooled to room temperature at a cooling rate of 10℃ / min. The alloy after billeting was heated to 700℃, heated at a rate of 50℃ / min, kept warm for 30min and then forged, forged once, with a total deformation of 20%, and then cooled to room temperature at a rate of 10℃ / min. Then, three rolling processes were carried out: the first rolling process was heated to 500℃, kept warm for 30min, the rolling deformation was 10%, rolled once, cooled to 100℃, and the cooling rate was 10℃ / min; the second rolling process was heated to 400℃, kept warm for 30min, rolled at 90°, the deformation was 10%, rolled once, cooled to room temperature, and the cooling rate was 10℃ / min; the third rolling process was heated to 200℃, kept warm for 30min, rolled at 90° again, the deformation was 10%, rolled once, cooled to room temperature, and the cooling rate was 10℃ / min to obtain the slab. The slab was cold rolled with a deformation of 10% to obtain a foil with a thickness of 0.12mm. The foil was rapidly heated to 700℃, the heating rate was 20℃ / min, kept warm for 5min, and then rapidly cooled to room temperature, and the cooling rate was 10℃ / min. The cooled foil was heated to 200°C at a rate of 50°C / min, kept warm for 10 minutes, cooled to 100°C and kept warm for 5 minutes at a cooling rate of 10°C / min, and then air-cooled to room temperature. The foil was straightened at a straightening temperature of 100°C, a straightening force of 50kN, and a strain of 0.05%. The straightened foil was heated to 200°C at a rate of 50°C / min, kept warm for 5 minutes, cooled to 100°C and kept warm for 5 minutes at a cooling rate of 10°C / min, and then air-cooled to room temperature. Room temperature aging treatment was performed for 1 day. The final titanium alloy foil did not meet the requirements in terms of technical parameters, resulting in its flexibility and strength not meeting expectations.
[0063] Comparative Example 3
[0064] Use sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide as raw materials for preliminary smelting, and adjust the composition content to the alloy element composition of Ti: 64.5%, Zr: 10%, Nb: 20%, Sn: 5%, O: 0.5%. After preliminary smelting, the alloy is pressed into alloy electrodes. The alloy electrodes are placed in a vacuum induction melting furnace and heated to a vacuum degree of not less than 10 -5Pa was melted twice to obtain an alloy ingot. The alloy ingot was heated to 750℃, kept warm for 45min, forged with a deformation of 20% and then cooled to room temperature at a cooling rate of 15℃ / min. The alloy after billeting was heated to 750℃, heated at a rate of 75℃ / min, kept warm for 45min and then forged, forged twice, with a total deformation of 30%, and then cooled to room temperature at a rate of 15℃ / min. The steel sheet was subjected to triple rolling: the first rolling was heated to 550°C, kept at this temperature for 45 minutes, the rolling deformation was 20%, the rolling was repeated for 2 passes, and the steel sheet was cooled to 150°C at a cooling rate of 20°C / min; the second rolling was heated to 450°C, kept at this temperature for 45 minutes, rolled at 90°, the deformation was 20%, the rolling was repeated for 2 passes, the steel sheet was cooled to room temperature at a cooling rate of 20°C / min; the third rolling was heated to 250°C, kept at this temperature for 45 minutes, rolled at 90° again, the deformation was 20%, the steel sheet was rolled for 2 passes, the steel sheet was cooled to room temperature at a cooling rate of 20°C / min, and the steel sheet was obtained by cold rolling with a deformation of 20% to obtain a foil with a thickness of 0.12 mm. The foil was rapidly heated to 750°C at a heating rate of 30°C / min, kept at this temperature for 10 minutes, and then rapidly cooled to room temperature at a cooling rate of 15°C / min. The cooled foil was heated to 300°C at a rate of 75°C / min, kept warm for 15 minutes, cooled to 200°C and kept warm for 5 minutes at a cooling rate of 15°C / min, and then air-cooled to room temperature. The foil was straightened at a straightening temperature of 150°C, a straightening force of 75kN, and a strain of 0.08%. The straightened foil was heated to 300°C at a rate of 75°C / min, kept warm for 10 minutes, cooled to 200°C and kept warm for 5 minutes at a cooling rate of 15°C / min, and then air-cooled to room temperature. Room temperature aging treatment was performed for 1.5 days. The final titanium alloy foil did not meet the requirements in terms of composition and technical parameters, resulting in its mechanical properties and flexibility not meeting expectations.
[0065] The high-flexibility and high-strength titanium alloy foil provided in Examples 1 to 8 is prepared by improving the processing technology, and has a strength of 710MPa to 1190MPa, an elastic strain of 1.1% to 2.0%, can be bent at least 50,000 times, and has a density not higher than 6.0g / cm 3 , which can well meet the application needs in the 3C field.
[0066] Table 1 Foil performance indicators
[0067]
[0068] The specific descriptions of the indicators in Table 1 are as follows:
[0069] Thickness: The technical requirement thickness range is 0.01mm~0.20mm, and the thickness of all examples meets the requirement. The thickness of comparative examples 1 and 2 is also within the technical requirement range.
[0070] Surface roughness (Ra): The technical requirement is that the surface roughness is 0.09-0.13, and the surface roughness of all examples meets the requirement. The surface roughness of Comparative Example 1, Comparative Example 2, and Comparative Example 3 are 0.20, 0.18, and 0.22, respectively, all exceeding the technical requirement.
[0071] Tensile strength: The technical requirement for tensile strength is 710MPa~1190MPa, and the tensile strength of all examples meets the requirement. The tensile strengths of Comparative Examples 1, 2, and 3 are 650MPa, 670MPa, and 680MPa, respectively, all lower than the technical requirement.
[0072] Elastic modulus: The technical requirement is that the elastic modulus is 41 GPa to 69 GPa, and the elastic moduli of all embodiments meet the requirement. The elastic moduli of Comparative Example 1, Comparative Example 2, and Comparative Example 3 are 75 GPa, 72 GPa, and 74 GPa, respectively, all of which are higher than the technical requirement.
[0073] Elastic strain: The technical requirement for elastic strain is 1.1% to 2.0%, and the elastic strains of all embodiments meet the requirement. The elastic strains of Comparative Examples 1, 2, and 3 are 1.0%, 1.1%, and 0.9%, respectively, and the elastic strains of Comparative Examples 1 and 3 are both lower than the technical requirement.
Claims
1. A method for preparing a high-flexibility, high-strength titanium alloy foil, wherein the alloy mass percentages satisfy: Ti: 57.5% to 69.95%, Nb: 22% to 26%, Zr: 2% to 6%, Sn: 6% to 10%, O: 0.05% to 0.5%; the thickness is 0.01 mm to 0.20 mm, and the surface roughness Ra is 0.09 μm to 0.13 μm; characterized in that, Follow these steps in order: Step 1: Raw material proportioning and preliminary smelting: Use sponge titanium, sponge zirconium, pure niobium, titanium-tin master alloy and titanium dioxide as raw materials for preliminary smelting, adjust the proportion of each component to form an alloy, and make the mass percentage of the element composition of the alloy meet the following requirements: Ti: 57.5%~69.95%, Nb: 22%~26%, Zr: 2%~6%, Sn: 6%~10%, O: 0.05%~0.5%; Step 2: Alloy electrode preparation: After preliminary smelting, the alloy is pressed into alloy electrodes; Step 3: Vacuum induction melting: Place the alloy electrode in a vacuum induction melting furnace and heat it in a vacuum degree of not less than 10 -5 Pa, the melting times are 2 to 4 times, and the alloy ingot is obtained; Step 4: Forging and blanking: heating and keeping the alloy ingot warm, then forging and blanking, and then cooling to room temperature; Step 5: Forging treatment: The alloy after billeting is heated, kept warm, forged and deformed, and then cooled to room temperature; Step 6: One room temperature aging treatment: Perform one room temperature aging treatment for 3 to 7 days; Step 7: Triple rolling: The forged alloy is triple rolled to obtain a slab; Step 8: Cold rolling: cold rolling the slab obtained in step 7, with a deformation amount of 30% to 95%, controlling the final thickness, and obtaining a foil with a thickness of 0.01 mm to 0.2 mm; Step 9: Rapid heating and cooling: The foil is quickly heated and then kept warm, and then cooled to room temperature at a controlled rate; Step 10: Preliminary heat treatment: The foil after rapid heating and cooling is heated and then kept warm, then cooled at a controlled rate and kept warm, and then air-cooled to room temperature; Step 11: Straightening treatment: Straightening treatment is performed on the foil after the preliminary heat treatment; Step 12: Secondary heat treatment: the straightened foil is heated and then kept warm, then cooled at a controlled rate and kept warm, and then air-cooled to room temperature; Step 13: Secondary room temperature aging treatment: Perform room temperature aging treatment for 1 to 3 days to obtain a titanium alloy foil with high flexibility and high strength; Among them, the triple rolling process is: First heavy rolling: the material is heated to 300℃~900℃ and then kept warm for 30min~120min, then the first heavy rolling is carried out, the number of rolling passes is 3~4, and after the rolling is completed, it is cooled to 0~400℃ and kept warm at a cooling rate of 25℃ / min~27℃ / min; the deformation of the first heavy rolling is 10%~40%; Second rolling: the material is heated to 300℃~700℃ and then kept warm for 30min~120min, then the material is reversed by 90° for the second rolling, with 4 passes, and then cooled to room temperature after the rolling, with a cooling rate of 25℃ / min~27℃ / min; among which, based on the material obtained after the first rolling, the deformation of the second rolling is 10%~40%; The third rolling: the material is heated to 20℃~400℃ and then kept warm for 30min~120min, then the direction is changed by 90° for the third rolling, the number of rolling passes is 3~5, and the material is cooled to room temperature after the rolling, and the cooling rate is 25℃ / min~27℃ / min; among them, based on the material obtained after the second rolling, the deformation of the third rolling is 10%~40%; In step 4, the specific process of forging and blanking is: heating the alloy ingot to 800°C~840°C, keeping the temperature for 60 minutes, forging and blanking with a deformation amount of 30%~35%, controlling the cooling rate to 20°C / min to 25°C / min after blanking, and cooling to room temperature; In step 5, the alloy after billeting is heated to 800°C~850°C at a rate of 100°C / min to 110°C / min, kept at this temperature for 60 minutes, and then forged for 3 times until the forging deformation is 50%~55%; After forging, the steel is cooled to room temperature at a rate of 20°C / min to 25°C / min; In step 9, the temperature is raised to 800°C to 880°C at a rate of 20°C / min to 100°C / min, and kept at this temperature for 10 to 20 minutes; then the temperature is rapidly cooled to room temperature at a cooling rate of 30 to 50°C / min; The preliminary heat treatment process is as follows: the cooled foil is heated to 250°C~450°C at a rate of 100°C / min, kept at this temperature for 1min to 20min, then cooled at a rate of 10°C / min to 25°C / min until the foil temperature is 100°C~120°C lower than the preliminary heat treatment temperature, kept at this temperature for 10min, and then air-cooled to room temperature; The secondary heat treatment process is as follows: the straightened foil is heated to 400-600°C at a rate of 100°C / min, kept at that temperature for 1-15min, then cooled at a rate of 30°C / min until the foil temperature is 100-250°C lower than the secondary heat treatment temperature, kept at that temperature for 1-30min, and then air-cooled to room temperature; In step 11, the straightening temperature is 20°C to 500°C, the straightening force is 100 kN to 500 kN, and the strain is 0.01% to 0.30%.
2. The method for preparing a high-flexibility, high-strength titanium alloy foil according to claim 1, characterized in that: The titanium alloy foil has a tensile strength of 710 MPa to 1190 MPa, an elastic modulus of 41 GPa to 69 GPa, and an elastic strain of 1.1% to 2.0% along any direction of the foil surface.
3. Application of the high-flexibility, high-strength titanium alloy foil prepared by the method according to any one of claims 1 to 2 in 3C electronic devices.
Citation Information
Patent Citations
Biomedical beta-titanium alloy material and preparation method
CN102899528A
Wide-temperature-range nonlinear elastic flexible alloy and preparation method thereof
CN117418139A
High-strength titanium-niobium-zirconium-tin alloy with extremely low resistance temperature coefficient and preparation method of titanium-niobium-zirconium-tin alloy
CN117867323A
Super elasticity low modulus titanium alloy and preparing and processing method
CN1648268A
Titanium material for manufacturing metal foil, method for manufacturing titanium material for manufacturing metal foil, and metal foil manufacturing drum