A high crack-resistant and anti-seepage mortar material and its preparation method and application

By using the design of polyester fiber-coated basalt fiber and rubber-coated ceramics in building mortar materials, combined with cement and epoxy resin, the problem of insufficient crack resistance and anti-permeability of existing mortar materials is solved, and efficient anti-crack properties are achieved. It has excellent cracking and impermeability properties, reduces costs, and is suitable for extreme environments.

CN118598624BActive Publication Date: 2024-10-01BEIJING ECO HOME (LETING) TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088334.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-01
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The crack resistance, anti-seepage and waterproof properties of existing building mortar materials cannot meet the needs of extreme environments, especially under extreme weather conditions with large humidity changes, which are prone to cracking or water seepage problems.

Method used

Cement and epoxy resin are used as cementing materials, combined with lime powder, standard sand, polyester fiber/polydopamine/basalt fiber composite materials and rubber-ceramic composite particles, and water reducing agents, dispersants and stabilizers are used as auxiliaries. Through the design of polyester fiber-coated basalt fiber and rubber-coated ceramic, a highly crack-resistant and impermeable mortar material is formed.

Benefits of technology

It significantly improves the crack resistance and impermeability of mortar materials, reduces preparation costs, provides excellent durability, and can meet the use requirements of extreme environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of building materials, and specifically discloses a high crack-resistant and anti-seepage mortar material and its preparation method and application. The high crack-resistant and anti-seepage mortar material includes the following raw material components by mass: 80-110 parts of cement, 50-70 parts of lime powder, 140-160 parts of standard sand, 1-2 parts of water reducer, 3-5 parts of dispersant, 0.05-0.1 parts of stabilizer, 35-60 parts of polyester fiber / polydopamine / basalt fiber composite material, 50-70 parts of rubber-ceramic composite particles, 30-50 parts of epoxy resin and 70-100 parts of water. The high crack-resistant and anti-seepage mortar material provided by the present invention has good crack resistance and anti-seepage performance and excellent durability, which can effectively solve the problem that the crack resistance and anti-seepage performance of the building mortar material in the prior art still cannot meet the environmental requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and specifically discloses a high-cracking and anti-seepage mortar material and a preparation method and application thereof. Background Art

[0002] Mortar materials are the most widely used construction materials today. With the vigorous development of the domestic construction industry, the requirements for the crack resistance, seepage resistance and waterproof performance of mortar materials used in the construction process are also constantly increasing. However, the current crack resistance and seepage resistance of mortar materials are far from meeting the needs of social development. Especially in recent years, extreme weather has occurred frequently and the humidity in the environment has changed greatly, which has caused mortar materials to crack or seep easily, causing great impact on people's living and working environment. Therefore, extensive research has been carried out at home and abroad on how to improve the crack resistance and seepage resistance of building mortar materials.

[0003] In the prior art, this problem is mostly solved by doping fiber-like substances or modifying the mortar components. However, fiber materials have high toughness but limited hardness, and modifying the components will lead to an increase in the cost of mortar materials. More importantly, even mortar materials that have been fiber-doped or component-modified still have problems with crack resistance and impermeability and waterproofing that cannot meet the needs of extreme environments. Therefore, the development of a highly crack-resistant and impermeable mortar material is of great significance for solving construction problems and improving people's living and working environment. Summary of the invention

[0004] In view of the problem that the crack resistance and impermeability of building mortar materials in the prior art still cannot meet environmental requirements, the present invention provides a high crack resistance and impermeability mortar material and its preparation method and application. The high crack resistance and impermeability mortar material is prepared with cement and epoxy resin as gelling materials; lime powder, standard sand, polyester fiber / polydopamine / basalt fiber composite materials and rubber-ceramic composite particles as aggregates; water reducer, dispersant and stabilizer as additives. The present invention utilizes the synergistic effect of each raw material component to make the obtained high crack resistance and impermeability mortar material have good crack resistance and impermeability and excellent durability.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The first aspect of the present invention provides a highly crack-resistant and anti-seepage mortar material, comprising the following raw material components in parts by weight: 80-110 parts of cement, 50-70 parts of lime powder, 140-160 parts of standard sand, 1-2 parts of water reducer, 3-5 parts of dispersant, 0.05-0.1 parts of stabilizer, 35-60 parts of polyester fiber / polydopamine / basalt fiber composite material, 50-70 parts of rubber-ceramic composite particles, 30-50 parts of epoxy resin and 70-100 parts of water.

[0007] Basalt fiber is an inorganic fiber with high strength, high chemical stability, corrosion resistance and high tensile strength, but it is relatively brittle, and its surface is smooth and not easy to react. Therefore, although the direct application of basalt fiber to mortar materials will improve the mechanical properties and stability of mortar materials to a certain extent, it will also cause the mortar materials to be brittle and their crack resistance is insufficient. The present invention designs a new composite fiber material based on basalt fiber, using polydopamine as a bridge to coat the surface of basalt fiber with better toughness. Dopamine can adhere to the surface of basalt fiber through polymerization reaction, and polydopamine has a large number of hydroxyl functional groups, which can be used as a bridge to graft polyester fiber materials containing carbonyl groups to firmly bond the two fibers together.

[0008] Polyester fiber has a linear structure, and its molecular chain contains both rigid groups and flexible groups, which also gives it a combination of rigid and flexible mechanical properties. The carbonyl group in the polyester fiber molecule can combine with the hydroxyl group in polydopamine and be grafted onto the surface of the basalt fiber to form a coating structure, thereby obtaining the polyester fiber / polydopamine / basalt fiber composite material. Since the flexible fiber is coated on the surface of the basalt fiber, the polyester fiber / polydopamine / basalt fiber composite material improves the toughness of the fiber and greatly reduces its brittleness, thereby improving the crack resistance of the mortar material. In addition, since the two are bonded by chemical bonds, the structure is denser, which improves the impermeability of the mortar material.

[0009] In addition, the present invention also designs a rubber-ceramic composite particle, which is made from waste ceramics and waste rubber powder as raw materials. The rubber-ceramic composite particle uses ceramic as a skeleton and rubber as a filling coating, and not only has the hardness of ceramics, but also has the flexibility and elasticity of rubber. This component can effectively improve the flexibility of the mortar material and reduce its risk of cracking. This material consumes a large amount of waste ceramics and waste rubber powder, effectively alleviating the processing pressure of these two solid wastes and reducing the preparation cost of the mortar material.

[0010] Furthermore, the present invention also adds raw material components such as epoxy resin and lime powder, so that the obtained mortar material not only has excellent crack resistance and anti-seepage performance, but also has good mechanical properties and durability. The technical solution of the present invention effectively solves the problem that the crack resistance and anti-seepage performance of building mortar materials in the prior art cannot meet environmental requirements, and provides new ideas and theoretical basis for building materials.

[0011] Preferably, the preparation method of the polyester fiber / polydopamine / basalt fiber composite material comprises the following steps:

[0012] S1, crushing the basalt fiber, heating it to 200°C-300°C for heat treatment, and obtaining pretreated basalt fiber;

[0013] S2, dispersing the pretreated basalt fiber in Tris-HCl buffer, adding dopamine, mixing evenly, performing hydrothermal reaction at 70° C.-90° C., and drying to obtain polydopamine-coated basalt fiber;

[0014] S3, dispersing the polyester fiber in an alcohol solution, adding a silane coupling agent and the polydopamine-coated basalt fiber, mixing evenly, performing a coupling reaction at 80° C.-100° C., filtering, and drying to obtain a polyester fiber / polydopamine / basalt fiber composite material.

[0015] Basalt fiber has a smooth surface and is not prone to chemical reactions. High-temperature treatment can improve its surface roughness, thereby increasing its surface chemical activity, which is conducive to polydopamine grafting modification. Dopamine can adhere to the surface of basalt fiber through polymerization reaction. Moreover, polydopamine has a large number of hydroxyl functional groups, which can be used as a bridge to graft polyester fiber materials containing carbonyl groups, firmly bonding the two fibers together.

[0016] Further preferably, in S1, the temperature is increased by programmed temperature increase at a rate of 10°C / min-20°C / min.

[0017] Further preferably, in S1, the heat treatment time is 2h-4h.

[0018] Further preferably, in S1, the length of the basalt fiber is 0.3 mm-0.5 mm.

[0019] Further preferably, in S2, the concentration of Tris in the Tris-HCl buffer is 9 mmol / L-12 mmol / L, and the pH is 6-7.

[0020] Further preferably, in S2, the mass volume ratio of the dopamine to the Tris-HCl buffer is 2g:1L-3g:2L.

[0021] Further preferably, in S2, the mass ratio of the pretreated basalt fiber to the dopamine is 1:0.2-2:0.3.

[0022] Further preferably, in S2, the hydrothermal reaction time is 10h-14h.

[0023] Further preferably, in S3, the alcohol solution is a 50%-75% ethanol solution.

[0024] Further preferably, in S3, the mass volume ratio of the polyester fiber to the alcohol solution is 1 g:3 mL-3 g:15 mL.

[0025] Further preferably, in S3, the silane coupling agent is KH-550.

[0026] Further preferably, in S3, the mass ratio of the polyester fiber to the polydopamine-coated basalt fiber is 1:2-1:3.

[0027] Further preferably, in S3, the amount of the silane coupling agent added is 5%-10% of the mass of the alcohol solution.

[0028] Further preferably, in S3, the coupling reaction time is 4h-6h.

[0029] Preferably, the method for preparing the rubber-ceramic composite particles comprises the following steps:

[0030] Step a, ball-milling the waste ceramics and performing a heat treatment at 100° C.-150° C. to obtain pretreated ceramic powder;

[0031] Step b: uniformly mixing the pretreated ceramic powder and the waste rubber powder, heating the mixture to 450° C.-550° C. for secondary heat treatment to obtain the rubber-ceramic composite particles.

[0032] Further preferably, in step a, the rotation speed of the ball mill is 500 rpm-800 rpm, and the ball milling time is 2 h-4 h.

[0033] Further preferably, in step a, the mass ratio of the pretreated ceramic powder to the waste rubber powder is 1:3-2:8.

[0034] Further preferably, in step a, the holding time of the primary heat treatment is 3h-6h.

[0035] Further preferably, in step b, the holding time of the secondary heat treatment is 4h-8h.

[0036] Further preferably, the primary heat treatment and the secondary heat treatment are both heated by programmed heating, and the heating rate of the primary heat treatment is 4°C / min-6°C / min; the heating rate of the secondary heat treatment is 10°C / min-20°C / min.

[0037] Preferably, the particle size of the rubber-ceramic composite particles is 0.3 mm-0.5 mm.

[0038] Preferably, the cement is Portland cement.

[0039] Preferably, the particle size of the lime powder is 0.1 mm-0.3 mm.

[0040] Preferably, the particle size of the standard sand is 0.2 mm-0.5 mm.

[0041] Preferably, the water reducer is any one of a sodium lignin sulfonate water reducer, a naphthalene-based high-efficiency water reducer, an aliphatic high-efficiency water reducer, an amino high-efficiency water reducer or a polycarboxylic acid high-efficiency water reducer.

[0042] Preferably, the dispersant is a fatty acid dispersant.

[0043] Preferably, the stabilizer is any one of EL0002, TAB-2 or T-386.

[0044] The second aspect of the present invention provides a method for preparing the highly crack-resistant and anti-seepage mortar material, comprising the following steps: weighing each raw material component according to the designed ratio, and mixing the weighed components evenly to obtain the highly crack-resistant and anti-seepage mortar material.

[0045] The third aspect of the present invention provides the use of the high crack-resistant and anti-seepage mortar material or the high crack-resistant and anti-seepage mortar material prepared by the preparation method of the high crack-resistant and anti-seepage mortar material in the field of building materials.

[0046] In summary, the present invention uses cement and epoxy resin as cementitious materials; lime powder, standard sand, polyester fiber / polydopamine / basalt fiber composite material and rubber-ceramic composite particles as aggregates; water reducer, dispersant and stabilizer as additives to prepare a high crack resistance and anti-seepage mortar material. The high crack resistance and anti-seepage mortar material has good crack resistance and anti-seepage performance and excellent durability. The use of the mortar material can effectively solve the problem that the crack resistance and anti-seepage performance of the building mortar material in the prior art still cannot meet the environmental requirements. DETAILED DESCRIPTION

[0047] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Example 1

[0049] This embodiment provides a high crack-resistant and anti-seepage mortar material and a preparation method thereof, which specifically includes the following contents:

[0050] The highly crack-resistant and anti-seepage mortar material includes the following raw material components in parts by weight: 100 parts of cement, 55 parts of lime powder, 140 parts of standard sand, 2 parts of sodium lignin sulfonate water reducer, 4 parts of fatty acid dispersant, 0.08 parts of TAB-2 stabilizer, 45 parts of polyester fiber / polydopamine / basalt fiber composite material, 60 parts of rubber-ceramic composite particles, 40 parts of epoxy resin and 90 parts of water.

[0051] Weigh each raw material component according to the designed proportion, mix each weighed component evenly, and obtain a highly crack-resistant and anti-seepage mortar material.

[0052] The preparation method of the polyester fiber / polydopamine / basalt fiber composite material comprises the following steps:

[0053] S1. 50 g of basalt fiber was crushed into a length of 0.4 mm, and the temperature was raised to 250° C. at a heating rate of 15° C. / min for heat treatment for 3 h to obtain pretreated basalt fiber;

[0054] S2, dispersing the pretreated basalt fiber in 5L of Tris-HCl buffer with a pH of 6.5 and a concentration of 10mmol / L, adding 10g of dopamine, ultrasonicating for 15min, performing hydrothermal reaction at 80°C for 12h, and drying at 70°C for 5h to obtain polydopamine-coated basalt fiber;

[0055] S3. Disperse 30 g of polyester fiber in 100 mL of 65% ethanol solution, add 5 g of KH-550 alkane coupling agent and the polydopamine-coated basalt fiber, ultrasonicate for 20 min, carry out coupling reaction at 90 ° C for 4 h, filter, and dry at 80 ° C for 2 h to obtain a polyester fiber / polydopamine / basalt fiber composite material.

[0056] The method for preparing the rubber-ceramic composite particles comprises the following steps:

[0057] Step a, ball milling 100 g of waste ceramic at a rotation speed of 700 rpm for 3 h, then heating to 130° C. at a heating rate of 5° C. / min, performing a heat treatment, and keeping the temperature for 4 h to obtain pretreated ceramic powder;

[0058] Step b: evenly mix the pretreated ceramic powder and 400 g of waste rubber powder, heat the mixture to 500° C. at a heating rate of 10° C. / min for secondary heat treatment, and keep the mixture warm for 5 hours to obtain the rubber-ceramic composite particles.

[0059] The cement is silicate cement; the particle size of the lime powder is 0.2 mm; and the particle size of the standard sand is 0.4 mm.

[0060] Example 2

[0061] This embodiment provides a high crack-resistant and anti-seepage mortar material and a preparation method thereof, which specifically includes the following contents:

[0062] The high crack-resistant and anti-seepage mortar material includes the following raw material components in parts by weight: 85 parts of cement, 60 parts of lime powder, 150 parts of standard sand, 1.5 parts of naphthalene-based high-efficiency water reducer, 3 parts of fatty acid dispersant, 0.1 parts of TAB-2 stabilizer, 50 parts of polyester fiber / polydopamine / basalt fiber composite material, 50 parts of rubber-ceramic composite particles, 50 parts of epoxy resin and 100 parts of water.

[0063] Weigh each raw material component according to the designed proportion, mix each weighed component evenly, and obtain a highly crack-resistant and anti-seepage mortar material.

[0064] The preparation method of the polyester fiber / polydopamine / basalt fiber composite material comprises the following steps:

[0065] S1. 50 g of basalt fiber was crushed into a length of 0.5 mm, and the temperature was raised to 300° C. at a heating rate of 20° C. / min for heat treatment for 2 h to obtain pretreated basalt fiber;

[0066] S2, dispersing the pretreated basalt fiber in 5L of Tris-HCl buffer with a pH of 6.5 and a concentration of 9mmol / L, adding 10g of dopamine, ultrasonicating for 15min, performing hydrothermal reaction at 90°C for 12h, and drying at 70°C for 5h to obtain polydopamine-coated basalt fiber;

[0067] S3. Disperse 30 g of polyester fiber in 100 mL of 60% ethanol solution, add 5 g of KH-550 alkane coupling agent and the polydopamine-coated basalt fiber, ultrasonicate for 20 min, carry out coupling reaction at 100 ° C for 5 h, filter, and dry at 80 ° C for 2 h to obtain a polyester fiber / polydopamine / basalt fiber composite material.

[0068] The method for preparing the rubber-ceramic composite particles comprises the following steps:

[0069] Step a, ball milling 100 g of waste ceramic at a speed of 600 rpm for 3.5 h, then heating to 100 ° C at a heating rate of 4 ° C / min, performing a heat treatment, and keeping the temperature for 6 h to obtain pretreated ceramic powder;

[0070] Step b: evenly mix the pretreated ceramic powder and 400 g of waste rubber powder, heat the mixture to 520° C. at a heating rate of 20° C. / min for secondary heat treatment, and keep the mixture warm for h to obtain the rubber-ceramic composite particles.

[0071] The cement is silicate cement; the particle size of the lime powder is 0.2 mm; and the particle size of the standard sand is 0.4 mm.

[0072] Example 3

[0073] This embodiment provides a high crack-resistant and anti-seepage mortar material and a preparation method thereof, which specifically includes the following contents:

[0074] The highly crack-resistant and anti-seepage mortar material includes the following raw material components in parts by weight: 110 parts of cement, 70 parts of lime powder, 140 parts of standard sand, 2 parts of polycarboxylic acid high-efficiency water reducing agent, 4 parts of fatty acid dispersant, 0.05 parts of TAB-2 stabilizer, 50 parts of polyester fiber / polydopamine / basalt fiber composite material, 60 parts of rubber-ceramic composite particles, 40 parts of epoxy resin and 90 parts of water.

[0075] Weigh each raw material component according to the designed proportion, mix each weighed component evenly, and obtain a highly crack-resistant and anti-seepage mortar material.

[0076] The preparation method of the polyester fiber / polydopamine / basalt fiber composite material comprises the following steps:

[0077] S1. 50 g of basalt fiber was crushed into a length of 0.4 mm, and the temperature was raised to 300° C. at a heating rate of 20° C. / min for heat treatment for 2 h to obtain pretreated basalt fiber;

[0078] S2, dispersing the pretreated basalt fiber in 5L of Tris-HCl buffer with a pH of 6.5 and a concentration of 10mmol / L, adding 10g of dopamine, ultrasonicating for 15min, performing hydrothermal reaction at 85°C for 12h, and drying at 70°C for 5h to obtain polydopamine-coated basalt fiber;

[0079] S3. Disperse 30 g of polyester fiber in 100 mL of 65% ethanol solution, add 5 g of KH-550 alkane coupling agent and the polydopamine-coated basalt fiber, ultrasonicate for 20 min, carry out coupling reaction at 80 ° C for 6 h, filter, and dry at 80 ° C for 2 h to obtain a polyester fiber / polydopamine / basalt fiber composite material.

[0080] The method for preparing the rubber-ceramic composite particles comprises the following steps:

[0081] Step a, ball milling 100 g of waste ceramic at a speed of 800 rpm for 2.5 h, then heating to 120° C. at a heating rate of 6° C. / min, performing a heat treatment, and keeping the temperature for 4 h to obtain pretreated ceramic powder;

[0082] Step b: evenly mix the pretreated ceramic powder and 400 g of waste rubber powder, heat the mixture to 550° C. at a heating rate of 10° C. / min for secondary heat treatment, and keep the mixture warm for 5 hours to obtain the rubber-ceramic composite particles.

[0083] The cement is silicate cement; the particle size of the lime powder is 0.2 mm; and the particle size of the standard sand is 0.4 mm.

[0084] Comparative Example 1

[0085] This comparative example provides a high crack resistance and impermeability mortar material and a preparation method thereof, which is different from Example 1 in that: the polyester fiber / polydopamine / basalt fiber composite material is replaced with an equal amount of basalt fiber material, and other components and processes remain unchanged, specifically including the following contents:

[0086] The high crack-resistant and anti-seepage mortar material includes the following raw material components in parts by mass: 100 parts of cement, 55 parts of lime powder, 140 parts of standard sand, 2 parts of sodium lignin sulfonate water reducer, 4 parts of fatty acid dispersant, 0.08 parts of TAB-2 stabilizer, 45 parts of basalt fiber material, 60 parts of rubber-ceramic composite particles, 40 parts of epoxy resin and 90 parts of water.

[0087] Weigh each raw material component according to the designed proportion, mix each weighed component evenly, and obtain a highly crack-resistant and anti-seepage mortar material.

[0088] The method for preparing the rubber-ceramic composite particles comprises the following steps:

[0089] Step a, ball milling 100 g of waste ceramic at a rotation speed of 700 rpm for 3 h, then heating to 130° C. at a heating rate of 5° C. / min, performing a heat treatment, and keeping the temperature for 4 h to obtain pretreated ceramic powder;

[0090] Step b: evenly mix the pretreated ceramic powder and 400 g of waste rubber powder, heat the mixture to 500° C. at a heating rate of 10° C. / min for secondary heat treatment, and keep the mixture warm for 5 hours to obtain the rubber-ceramic composite particles.

[0091] The cement is silicate cement; the particle size of the lime powder is 0.2 mm; and the particle size of the standard sand is 0.4 mm.

[0092] Comparative Example 2

[0093] This comparative example provides a high crack resistance and impermeability mortar material and a preparation method thereof, which is different from Example 1 in that: the polyester fiber / polydopamine / basalt fiber composite material is replaced with an equal amount of polyester fiber material, and other components and processes remain unchanged, specifically including the following contents:

[0094] The high crack-resistant and anti-seepage mortar material includes the following raw material components in parts by weight: 100 parts of cement, 55 parts of lime powder, 140 parts of standard sand, 2 parts of sodium lignin sulfonate water reducer, 4 parts of fatty acid dispersant, 0.08 parts of TAB-2 stabilizer, 45 parts of polyester fiber material, 60 parts of rubber-ceramic composite particles, 40 parts of epoxy resin and 90 parts of water.

[0095] Weigh each raw material component according to the designed proportion, mix each weighed component evenly, and obtain a highly crack-resistant and anti-seepage mortar material.

[0096] The method for preparing the rubber-ceramic composite particles comprises the following steps:

[0097] Step a, ball milling 100 g of waste ceramic at a rotation speed of 700 rpm for 3 h, then heating to 130° C. at a heating rate of 5° C. / min, performing a heat treatment, and keeping the temperature for 4 h to obtain pretreated ceramic powder;

[0098] Step b: evenly mix the pretreated ceramic powder and 400 g of waste rubber powder, heat the mixture to 500° C. at a heating rate of 10° C. / min for secondary heat treatment, and keep the mixture warm for 5 hours to obtain the rubber-ceramic composite particles.

[0099] The cement is silicate cement; the particle size of the lime powder is 0.2 mm; and the particle size of the standard sand is 0.4 mm.

[0100] Comparative Example 3

[0101] This comparative example provides a high crack-resistant and anti-seepage mortar material and a preparation method thereof, which is different from Example 1 in that the rubber-ceramic composite particles are replaced with an equal amount of ceramic particles, and other components and processes remain unchanged, specifically including the following contents:

[0102] The highly crack-resistant and anti-seepage mortar material includes the following raw material components in parts by weight: 100 parts of cement, 55 parts of lime powder, 140 parts of standard sand, 2 parts of sodium lignin sulfonate water reducer, 4 parts of fatty acid dispersant, 0.08 parts of TAB-2 stabilizer, 45 parts of polyester fiber / polydopamine / basalt fiber composite material, 60 parts of ceramic particles, 40 parts of epoxy resin and 90 parts of water.

[0103] Weigh each raw material component according to the designed proportion, mix each weighed component evenly, and obtain a highly crack-resistant and anti-seepage mortar material.

[0104] The preparation method of the polyester fiber / polydopamine / basalt fiber composite material comprises the following steps:

[0105] S1. 50 g of basalt fiber was crushed into a length of 0.4 mm, and the temperature was raised to 250° C. at a heating rate of 15° C. / min for heat treatment for 3 h to obtain pretreated basalt fiber;

[0106] S2, dispersing the pretreated basalt fiber in 5L of Tris-HCl buffer with a pH of 6.5 and a concentration of 10mmol / L, adding 10g of dopamine, ultrasonicating for 15min, performing hydrothermal reaction at 80°C for 12h, and drying at 70°C for 5h to obtain polydopamine-coated basalt fiber;

[0107] S3. Disperse 30 g of polyester fiber in 100 mL of 65% ethanol solution, add 5 g of KH-550 alkane coupling agent and the polydopamine-coated basalt fiber, ultrasonicate for 20 min, carry out coupling reaction at 90 ° C for 4 h, filter, and dry at 80 ° C for 2 h to obtain a polyester fiber / polydopamine / basalt fiber composite material.

[0108] The cement is silicate cement; the particle size of the lime powder is 0.2 mm; and the particle size of the standard sand is 0.4 mm.

[0109] In order to further reflect the technical effect of the present invention, the present invention conducted the following tests on the mortar materials obtained in Examples 1-3 and Comparative Examples 1-3: the compressive strength was tested with reference to the standard of GB / T17671-2021, and the anti-permeability performance test was performed with reference to the relevant procedures of the "Standard for Test Methods for Basic Performance of Building Mortar" (JGJ / T70-2009); the crack resistance test was performed with reference to the relevant procedures of the "Test Method for Cracking Resistance of Cement Mortar" (JCT951-2005); the results are shown in Table 1.

[0110] Table 1 Performance test results of various mortar materials

[0111]

[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A highly crack-resistant and impermeable mortar material, characterized in that: The raw material components include the following parts by weight: 80-110 parts of cement, 50-70 parts of lime powder, 140-160 parts of standard sand, 1-2 parts of water reducer, 3-5 parts of dispersant, 0.05-0.1 parts of stabilizer, 35-60 parts of polyester fiber / polydopamine / basalt fiber composite material, 50-70 parts of rubber-ceramic composite particles, 30-50 parts of epoxy resin and 70-100 parts of water; The preparation method of the polyester fiber / polydopamine / basalt fiber composite material comprises the following steps: S1, crushing the basalt fiber, heating it to 200°C-300°C for heat treatment, and obtaining pretreated basalt fiber; S2, dispersing the pretreated basalt fiber in Tris-HCl buffer, adding dopamine, mixing evenly, performing hydrothermal reaction at 70° C.-90° C., and drying to obtain polydopamine-coated basalt fiber; S3, dispersing the polyester fiber in an alcohol solution, adding a silane coupling agent and the polydopamine-coated basalt fiber, mixing evenly, performing a coupling reaction at 80° C.-100° C., filtering, and drying to obtain a polyester fiber / polydopamine / basalt fiber composite material; The method for preparing the rubber-ceramic composite particles comprises the following steps: Step a, ball-milling the waste ceramics and performing a heat treatment at 100° C.-150° C. to obtain pretreated ceramic powder; Step b, mixing the pretreated ceramic powder and the waste rubber powder uniformly, heating to 450° C.-550° C. for secondary heat treatment to obtain the rubber-ceramic composite particles; The dispersant is a fatty acid dispersant.

2. The high crack-resistant and anti-seepage mortar material according to claim 1, characterized in that: In S1, the temperature is increased by programmed temperature increase, and the rate of temperature increase is 10°C / min-20°C / min; In S1, the heat treatment time is 2h-4h; In S1, the length of the basalt fiber is 0.3 mm-0.5 mm.

3. The high crack-resistant and anti-seepage mortar material according to claim 1, characterized in that: In S2, the concentration of Tris in the Tris-HCl buffer is 9 mmol / L-12 mmol / L, and the pH is 6-7; In S2, the mass volume ratio of the dopamine to the Tris-HCl buffer is 2 g:1 L-3 g:2 L; In S2, the mass ratio of the pretreated basalt fiber to the dopamine is 1:0.2-2:0.3; In S2, the hydrothermal reaction time is 10h-14h.

4. The high crack-resistant and anti-seepage mortar material according to claim 1, characterized in that: In S3, the alcohol solution is a 50%-75% ethanol solution; In S3, the mass volume ratio of the polyester fiber to the alcohol solution is 1 g:3 mL-3 g:15 mL; In S3, the silane coupling agent is KH-550.

5. The high crack-resistant and anti-seepage mortar material according to claim 1, characterized in that: In S3, the mass ratio of the polyester fiber to the polydopamine-coated basalt fiber is 1:2-1:3; In S3, the amount of the silane coupling agent added is 5%-10% of the mass of the alcohol solution; In S3, the coupling reaction time is 4h-6h.

6. The high crack-resistant and impermeable mortar material according to claim 1, characterized in that: In step a, the ball milling speed is 500 rpm-800 rpm, and the ball milling time is 2 h-4 h; In step b, the mass ratio of the pretreated ceramic powder to the waste rubber powder is 1:3-2:8; In step a, the holding time of the primary heat treatment is 3h-6h; In step b, the holding time of the secondary heat treatment is 4h-8h; The primary heat treatment and the secondary heat treatment are both heated by programmed heating, the heating rate of the primary heat treatment is 4°C / min-6°C / min; the heating rate of the secondary heat treatment is 10°C / min-20°C / min.

7. The method for preparing a highly crack-resistant and impermeable mortar material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: weighing various raw material components according to the designed proportion, and uniformly mixing the weighed components to obtain a high crack-resistant and anti-seepage mortar material.

8. Use of the highly crack-resistant and anti-seepage mortar material according to any one of claims 1 to 6 or the highly crack-resistant and anti-seepage mortar material prepared by the preparation method of the highly crack-resistant and anti-seepage mortar material according to claim 7 in the field of building materials.