Fuel cell membrane electrode and preparation method thereof
By using the combination technology of carbon nanotubes and PFSA ionomers in fuel cell membrane electrodes, a long-range continuous ionomer network is constructed, which solves the problem of poor continuity of proton and electron transport networks in traditional membrane electrodes, and realizes efficient catalysts Utilized and low-cost preparation process.
Patent Information
- Application Number
- CN202410838350.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-26
AI Technical Summary
In the traditional fuel cell membrane electrode preparation process, the proton transmission network in the cathode catalytic layer has poor continuity, resulting in high proton transmission impedance, poor continuity of the electron transmission network, low catalyst utilization, and high maintenance cost and poor safety of the preparation system.
By mixing carbon nanotubes with sulfuric acid, loading platinum particles, diluting PFSA ionomer solution with isopropanol for impregnation treatment, nano-level ionomer self-assembly is achieved, and a long-range continuous ionomer network framework is constructed, combining with Ultrasonic treatment and magnetic stirring were used to prepare efficient membrane electrodes.
It improves catalyst utilization, reduces proton and electron transport impedance, simplifies the preparation process, reduces costs, and improves the performance and safety of membrane electrodes.
Smart Images

Figure CN118610485B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of fuel cells, and in particular relates to a fuel cell membrane electrode and a preparation method thereof. Background Art
[0002] In the membrane electrode of a proton exchange membrane fuel cell, oxygen reaches the reaction site on the cathode side and undergoes an ORR reaction to generate O 2- , hydrogen enters the anode side and undergoes HRR reaction to generate H + The ionomer network on the cathode side passes through the proton exchange membrane and reaches the cathode reaction site, where it reacts with the generated O 2- Combined with generated water, the battery power generation process is completed. In this process, the proton transmission resistance in the ionomer network on the cathode side is large, which is an important source of overpotential loss in low-load cathode fuel cells. At present, commercial ionomers are perfluorosulfonic acid type (PFSA), which consists of a hydrophobic main chain (-CF4) and hydrophilic side chain sulfonic acid groups. Its hydrophobic main chain provides mechanical strength for the ionomer skeleton, while the sulfonic acid group provides a place for proton conduction. Therefore, ensuring the continuity of the cathode catalyst layer ionomer network and ensuring its sufficient hydration are the key to achieving its proton conduction.
[0003] However, during the slurry mixing process, the sulfur element in the sulfonic acid group of the PFSA ionomer side chain will spontaneously form a Pt-S bond with the catalyst active phase Pt particles. The adsorption strength of this chemical bond is much higher than the interaction between the ionomer and the carbon carrier. As a result, in the prepared catalytic layer, there is often a serious ionomer agglomeration problem on the surface of the Pt particles, while there is a discontinuous ionomer film on the surface of the carbon carrier. In this way, continuous ionomer channels cannot be formed between Pt particles, resulting in the inactivation of a large number of Pt sites, a decrease in catalyst utilization, and high proton transfer impedance. At the same time, in the slurry obtained by the traditional preparation scheme, the Pt / C catalyst particles are small in size and high in surface energy. During the slurry mixing process, it is very easy to form 200-500 nanometer agglomerates, and the outer layer of these agglomerates is tightly wrapped by the ionomer, which makes the prepared cathode catalyst layer have poor continuity of electron transmission channels and low catalyst utilization.
[0004] Although the solution proposed in the Chinese patent application number CN201110251507.0 can indeed provide carbon nanotubes as catalyst carriers for the cathode of proton exchange membrane fuel cells, the patent is mainly aimed at improving the preparation efficiency, consistency and reducing equipment costs in the large-scale preparation process of carbon nanotube carriers. The carbon nanotube carriers prepared by it can achieve long-range continuous electron transmission in the cathode catalyst layer, but the continuity of the proton transmission channel in the obtained catalyst layer cannot be improved, and the problem of poor proton conductivity in the cathode catalyst layer has not been solved.
[0005] The Chinese patent with application number CN202310246660.7 proposes a solution to prepare a new membrane electrode through electrospinning technology, with the aim of improving catalyst utilization, and it is found that the electrode exhibits higher mass transfer performance. However, this method relies heavily on expensive electrospinning equipment. At the same time, a large amount of organic solvents that do not allow proton conduction are required in the electrospinning slurry as a binder to form an electrospinning slurry. These organic solvents still exist stably after the electrode is prepared. Although the cathode side of the obtained membrane electrode realizes a continuous proton transfer network, the proton conductivity of the network itself is sacrificed. Although the catalyst utilization rate is improved, the ohmic loss of the cathode catalyst layer is increased in turn.
[0006] The Chinese patent application number CN200510048034.9 proposed a new membrane electrode preparation scheme. The key components in the cathode catalyst layer are arranged in a directional and orderly manner by using multi-physical field induction such as heat, electricity, and magnetic field. However, this method relies heavily on expensive self-built electrode preparation equipment, and the electric field strength needs to be maintained at more than 4*10 5 V / m for at least 24 hours, which has extremely high safety risks and preparation costs. At the same time, this method can only further improve the performance of membrane electrodes at higher Pt loadings (>0.5mg / cm 2 Pt loading), without achieving increased utilization and performance for lower Pt loadings. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a fuel cell membrane electrode and a preparation method thereof.
[0008] The present invention is achieved through the following technical solutions.
[0009] The present invention provides a method for preparing a fuel cell membrane electrode, comprising the following steps:
[0010] S1: Mix carbon nanotubes and sulfuric acid, stir and heat the solution, add NaMnO4 and continue stirring, inject water after stirring, add hydrogen peroxide solution, wash the obtained product with water, centrifuge, precipitate and dry to obtain solid A;
[0011] S2: loading platinum particles onto the surface of solid A to obtain catalyst B;
[0012] S3: diluting the PFSA ionomer solution with isopropanol to obtain solution C, placing catalyst B in solution C, stirring, centrifuging and washing the product repeatedly until the supernatant is clear, and drying to obtain product solid particles D, then placing solid particles D in solution C and stirring, centrifuging, washing, and drying the product to obtain solid particles E;
[0013] S4: The solid particles E are mixed with water and isopropanol, and after ultrasonic treatment, a slurry is obtained. The slurry is sprayed as cathode slurry on the other side of the proton exchange membrane on the prepared anode side to obtain a membrane electrode, and finally dried.
[0014] Preferably, in step S1, the carbon nanotubes and sulfuric acid with a concentration of 0.5-1.5M are mixed, the rotor speed is adjusted to 1200rpm at room temperature, and the mixture is stirred at a constant speed for 12-36h until a homogeneous black viscous solution is formed; NaMnO4 is slowly added during the heating process until the heating is completed, and the stirring is continued for 12-36h. After the stirring is completed, deionized water is injected, and then a hydrogen peroxide solution with a mass concentration of 2-6% is added. During the liquid preparation process, the rotor speed is adjusted to 1200rpm, and stirring is maintained. After the reaction is complete, the solution is allowed to stand for 12 hours, and the obtained product is repeatedly washed with deionized water, centrifuged, precipitated, and dried after the supernatant is clarified.
[0015] Preferably, in step S2, after the formaldehyde solution and chloroplatinic acid solution with a mass concentration of 40-60% are mixed with solid A, deionized water is added and stirred for 10-50 minutes, ultrasonicated for 0.5-3 hours, condensed and refluxed for 2-8 hours in an oil bath environment of 100-140°C, placed for 10-20 hours to allow the solution to cool naturally, and treated by step A to obtain catalyst B. Step A comprises the following steps: after the solution cools naturally, it is filtered with a 0.1 micron microporous filter membrane, the product is repeatedly washed with deionized water until the filtrate is neutral, dried in a vacuum oven at 30-60°C for 18-30 hours, and ground and sieved after it cools naturally.
[0016] Preferably, in step S3, the PFSA ionomer solution with an initial mass concentration of 20% is diluted with isopropanol to a mass concentration of 0.15-0.35% to obtain solution C, the catalyst B is placed in solution C, magnetically stirred for 20-40 hours, the product is repeatedly centrifuged and washed until the supernatant is clear, and dried to obtain product solid particles D, and then the solid particles D are placed in the diluted solution C and magnetically stirred for 20-40 hours, the product is repeatedly centrifuged and washed until the supernatant is clear, and dried to obtain product solid particles E.
[0017] Preferably, in step S4, the obtained solid particles E are mixed with deionized water and isopropanol in a mass ratio of 1:10-40:100-300, ultrasonicated for 5-20 hours, and then sprayed.
[0018] Preferably, in step S1, after stirring, the solution is heated to 70-110°C at a rate of 1-5°C / s.
[0019] Preferably, in step S4, the obtained membrane electrode is placed in a vacuum oven at 30-60° C. and dried for not less than 3 hours.
[0020] A membrane electrode prepared by the method for preparing a fuel cell membrane electrode as described above, and a fuel cell prepared using the membrane electrode.
[0021] The beneficial effects of the present invention are:
[0022] 1. The present invention solves the problem that in the traditional membrane electrode preparation process, the proton transport ionomer network in the cathode catalyst layer is highly dependent on the intrinsic dispersion characteristics of the slurry, resulting in low continuity of the proton transport network, low catalyst utilization in the cathode catalyst layer, and high proton transport impedance; the present invention directly uses the PFSA ionomer self-assembly method to construct a long-range continuous ionomer network skeleton, thereby improving the catalyst utilization and reducing the proton transport impedance.
[0023] 2. The present invention solves the problem that in the traditional membrane electrode preparation process, the electron transport in the cathode catalyst layer is highly dependent on the intrinsic dispersion characteristics of the Pt / C catalyst agglomerates, resulting in poor continuity of the electron transport network, low catalyst utilization in the cathode catalyst layer, and high electron transport impedance; the present invention introduces carbon nanotubes as a new catalyst carrier, realizes long-range continuous electron transport, improves catalyst utilization, and reduces electron transport impedance.
[0024] 3. The present invention does not rely on expensive and complex electrode preparation systems to perform ordered electrode preparation operations, thus solving the problems of high maintenance costs and poor safety of traditional fuel cell membrane electrode preparation systems. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a schematic diagram of solid A of the present invention;
[0026] Figure 2 is a schematic diagram of catalyst B of the present invention;
[0027] Figure 3 is a schematic diagram of a solid particle E of the present invention;
[0028] Figure 4 It is a schematic diagram of the results of proton impedance measurement by the hydrogen pump method of the membrane electrode of the present invention and the prior art;
[0029] Figure 5 It is a schematic diagram of the results of measuring the electron transfer impedance of the membrane electrode of the present invention and the prior art using high-frequency impedance spectra;
[0030] Figure 6 Schematic diagram of comparison of the electrochemical effective area of the cathode side of the membrane electrode of the present invention and the membrane electrode of the prior art at the same cathode platinum loading;
[0031] Figure 7 Schematic diagram of performance comparison between the membrane electrode of the present invention and the prior art at the same cathode platinum loading; DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.
[0033] Embodiment 1:
[0034] like Figures 1 to 3 As shown, a method for preparing a fuel cell membrane electrode comprises the following steps:
[0035] S1: Mix carbon nanotubes and sulfuric acid, stir and heat the solution, add NaMnO4 and continue stirring, inject water after stirring, add hydrogen peroxide solution, wash the obtained product with deionized water repeatedly, centrifuge, precipitate and dry to obtain solid A. This step modifies the carbon nanotubes to adjust their properties so that they can be easily loaded by the active phase;
[0036] S2: loading platinum particles onto the surface of solid A to obtain catalyst B. In this step, the catalytically active phase, i.e., platinum particles, are loaded onto the surface of carbon nanotubes to obtain Pt / CNT catalyst particles, i.e., catalyst B.
[0037] S3: dilute the PFSA ionomer solution with isopropanol to obtain solution C, place catalyst B in solution C, stir vigorously magnetically, centrifuge and wash the product repeatedly until the supernatant is clear, and then dry to obtain solid particles D, then place solid particles D in solution C and stir vigorously magnetically, centrifuge and wash the product repeatedly to obtain solid particles E. This step of immersion operation realizes the nano-level "layer-by-layer self-assembly" of ionomers on the surface of Pt / CNT catalysts;
[0038] S4: Mix the solid particles E with water and isopropanol, and after ultrasonic treatment, spray the slurry as cathode slurry on the other side of the proton exchange membrane on which the common anode side has been prepared to obtain a membrane electrode, and finally dry it. This step sprays the cathode to prepare a proton exchange membrane fuel cell membrane electrode.
[0039] In the step S1, 10 g of carbon nanotubes and 100 mL of 0.5 M sulfuric acid are added to a 250 mL three-necked flask and mixed. The rotor speed is adjusted to 1200 rpm at room temperature, and the mixture is stirred at a constant speed for 12 hours until a homogeneous black viscous solution is formed. NaMnO4 is slowly added during the heating process until the heating is completed, and the stirring is continued for 12 hours. After the stirring is completed, the obtained liquid is transferred to a larger reaction container, 1 L of deionized water is injected, and then 100 mL of a 2% hydrogen peroxide solution is added. During the liquid preparation process, the rotor speed is adjusted to 1200 rpm, and the stirring is maintained. After the reaction is complete, the solution is allowed to stand overnight, and the obtained product is repeatedly washed with deionized water, centrifuged, and precipitated, and the supernatant is clarified and then dried.
[0040] In the step S2, 20 mL of 40% mass concentration formaldehyde solution, 50 mL of chloroplatinic acid solution and 10 g of solid A are mixed, and deionized water is added until the total volume is 300 mL, and stirred for 10 minutes. After ultrasonication for 0.5 hours, the mixture is condensed and refluxed in an oil bath environment at 100° C. for 2 hours, and the solution is allowed to cool naturally for 10 hours, and the catalyst B is obtained by treatment in step A.
[0041] In the step S3, 20% PFSA ionomer solution is diluted with isopropanol to a mass concentration of 0.15% to obtain 20 mL of solution C, 10 g of catalyst B is placed in 20 mL of solution C, and strongly magnetically stirred for 20 h. The product is repeatedly centrifuged and washed until the supernatant is clear, and then dried to obtain product solid particles D. 10 g of solid particles D are placed in the diluted 20 mL of solution C and strongly magnetically stirred for 20 h. The product is repeatedly centrifuged and washed until the supernatant is clear, and then dried to obtain product solid particles E loaded with long-range continuous ionomer film.
[0042] In the step S4, the obtained solid particles E are mixed with deionized water and isopropanol in a mass ratio of 1:10:100, ultrasonicated for 5 hours, and then sprayed.
[0043] In the step S1, after stirring, the solution is heated to 70°C at a rate of 1°C / s.
[0044] The step A comprises the following steps: after the solution is cooled naturally, the solution is filtered with a 0.1 micron microporous filter membrane, the product is repeatedly washed with deionized water until the filtrate is neutral, dried in a vacuum oven at 30° C. for 18 hours, and ground and sieved with a mortar after the solution is cooled naturally.
[0045] In the step S4, the obtained membrane electrode is placed in a vacuum oven at 30° C. and dried for 3.5 hours to completely evaporate the dispersed solvent in the anode and cathode catalyst layers to prepare the ordered membrane electrode.
[0046] Embodiment 2:
[0047] like Figures 1 to 3 As shown, a method for preparing a fuel cell membrane electrode comprises the following steps:
[0048] S1: Mix carbon nanotubes and sulfuric acid, stir and heat the solution, add NaMnO4 and continue stirring, inject water after stirring, add hydrogen peroxide solution, wash the obtained product with deionized water repeatedly, centrifuge, precipitate and dry to obtain solid A. This step modifies the carbon nanotubes to adjust their properties so that they can be easily loaded by the active phase;
[0049] S2: loading platinum particles onto the surface of solid A to obtain catalyst B. In this step, the catalytically active phase, i.e., platinum particles, are loaded onto the surface of carbon nanotubes to obtain Pt / CNT catalyst particles, i.e., catalyst B.
[0050] S3: dilute the PFSA ionomer solution with isopropanol to obtain solution C, place catalyst B in solution C, stir vigorously magnetically, centrifuge and wash the product repeatedly until the supernatant is clear, and then dry to obtain solid particles D, then place solid particles D in solution C and stir vigorously magnetically, centrifuge and wash the product repeatedly to obtain solid particles E. This step of immersion operation realizes the nano-level "layer-by-layer self-assembly" of ionomers on the surface of Pt / CNT catalysts;
[0051] S4: Mix the solid particles E with water and isopropanol, and after ultrasonic treatment, spray the slurry as cathode slurry on the other side of the proton exchange membrane on which the common anode side has been prepared to obtain a membrane electrode, and finally dry it. This step sprays the cathode to prepare a proton exchange membrane fuel cell membrane electrode.
[0052] In the step S1, 10 g of carbon nanotubes and 100 mL of 1.5 M sulfuric acid are added to a 250 mL three-necked flask and mixed. The rotor speed is adjusted to 1200 rpm at room temperature, and the mixture is stirred at a constant speed for 36 hours until a homogeneous black viscous solution is formed. NaMnO4 is slowly added during the heating process until the heating is completed, and the stirring is continued for 36 hours. After the stirring is completed, the obtained liquid is transferred to a larger reaction container, 1 L of deionized water is injected, and then 100 mL of a 6% hydrogen peroxide solution is added. During the liquid preparation process, the rotor speed is adjusted to 1200 rpm, and the stirring is maintained. After the reaction is complete, the solution is allowed to stand overnight, and the obtained product is repeatedly washed with deionized water, centrifuged, and precipitated, and the supernatant is clarified and then dried.
[0053] In the step S2, 20 mL of a 60% mass concentration formaldehyde solution, 50 mL of a chloroplatinic acid solution and 10 g of solid A are mixed, and deionized water is added until the total volume is 300 mL, and the mixture is stirred for 50 min. After ultrasonic treatment for 0.5-3 h, the mixture is condensed and refluxed in an oil bath at 140° C. for 8 h, and the solution is allowed to cool naturally for 20 h, and the catalyst B is obtained by treatment in step A.
[0054] In the step S3, 20% PFSA ionomer solution is diluted with isopropanol to a mass concentration of 0.35% to obtain 20 mL of solution C, 10 g of catalyst B is placed in 20 mL of solution C, and strongly magnetically stirred for 40 hours. The product is repeatedly centrifuged and washed until the supernatant is clear, and then dried to obtain product solid particles D. 10 g of solid particles D are placed in the diluted 20 mL of solution C and strongly magnetically stirred for 40 hours. The product is repeatedly centrifuged and washed until the supernatant is clear, and then dried to obtain product solid particles E loaded with long-range continuous ionomer film.
[0055] In the step S4, the obtained solid particles E are mixed with deionized water and isopropanol in a mass ratio of 1:40:300, ultrasonicated for 20 hours, and then sprayed.
[0056] In the step S1, after stirring, the solution is heated to 110°C at a rate of 5°C / s.
[0057] The step A comprises the following steps: after the solution is cooled naturally, the solution is filtered with a 0.1 micron microporous filter membrane, the product is repeatedly washed with deionized water until the filtrate is neutral, dried in a vacuum oven at 60° C. for 30 hours, and ground and sieved with a mortar after the solution is cooled naturally.
[0058] In the step S4, the obtained membrane electrode is placed in a vacuum oven at 60° C. and dried for 4 hours to completely evaporate the dispersed solvent in the anode and cathode catalyst layers to prepare the ordered membrane electrode.
[0059] Embodiment 3:
[0060] like Figures 1 to 3 As shown, a method for preparing a fuel cell membrane electrode comprises the following steps:
[0061] S1: Mix carbon nanotubes and sulfuric acid, stir and heat the solution, add NaMnO4 and continue stirring, inject water after stirring, add hydrogen peroxide solution, wash the obtained product with deionized water repeatedly, centrifuge, precipitate and dry to obtain solid A. This step modifies the carbon nanotubes to adjust their properties so that they can be easily loaded by the active phase;
[0062] S2: loading platinum particles onto the surface of solid A to obtain catalyst B. In this step, the catalytically active phase, i.e., platinum particles, are loaded onto the surface of carbon nanotubes to obtain Pt / CNT catalyst particles, i.e., catalyst B.
[0063] S3: dilute the PFSA ionomer solution with isopropanol to obtain solution C, place catalyst B in solution C, stir vigorously magnetically, centrifuge and wash the product repeatedly until the supernatant is clear, and then dry to obtain solid particles D, then place solid particles D in solution C and stir vigorously magnetically, centrifuge and wash the product repeatedly to obtain solid particles E. This step of immersion operation realizes the nano-level "layer-by-layer self-assembly" of ionomers on the surface of Pt / CNT catalysts;
[0064] S4: Mix the solid particles E with water and isopropanol, and after ultrasonic treatment, spray the slurry as cathode slurry on the other side of the proton exchange membrane on which the common anode side has been prepared to obtain a membrane electrode, and finally dry it. This step sprays the cathode to prepare a proton exchange membrane fuel cell membrane electrode.
[0065] In the step S1, 10 g of carbon nanotubes and 100 mL of 1 M sulfuric acid are added to a 250 mL three-necked flask and mixed. The rotor speed is adjusted to 1200 rpm at room temperature, and the mixture is stirred at a constant speed for 24 hours until a homogeneous black viscous solution is formed. NaMnO4 is slowly added during the heating process until the heating is completed, and the stirring is continued for 24 hours. After the stirring is completed, the obtained liquid is transferred to a larger reaction container, 1 L of deionized water is injected, and then 100 mL of a 5% hydrogen peroxide solution is added. During the liquid preparation process, the rotor speed is adjusted to 1200 rpm, and the stirring is maintained. After the reaction is complete, the solution is allowed to stand overnight, and the obtained product is repeatedly washed with deionized water, centrifuged, and precipitated, and the supernatant is clarified and then dried.
[0066] In the step S2, 20 mL of 50% mass concentration formaldehyde solution, 50 mL of chloroplatinic acid solution and 10 g of solid A are mixed, and deionized water is added until the total volume is 300 mL, and stirred for 10-50 min. After ultrasonic treatment for 1 h, the mixture is condensed and refluxed in an oil bath at 120° C. for 5 h, and the solution is allowed to cool naturally for 15 h, and the catalyst B is obtained by treatment in step A.
[0067] In the step S3, 20% PFSA ionomer solution is diluted with isopropanol to a mass concentration of 0.25% to obtain 20 mL of solution C, 10 g of catalyst B is placed in 20 mL of solution C, and strongly magnetically stirred for 24 hours. The product is repeatedly centrifuged and washed until the supernatant is clear, and dried to obtain product solid particles D. 10 g of solid particles D are placed in the diluted 20 mL of solution C and strongly magnetically stirred for 24 hours. The product is repeatedly centrifuged and washed until the supernatant is clear, and then dried to obtain product solid particles E loaded with long-range continuous ionomer film.
[0068] In the step S4, the obtained solid particles E are mixed with deionized water and isopropanol in a mass ratio of 1:20:200, ultrasonicated for 10 hours, and then sprayed.
[0069] In the step S1, after stirring, the solution is heated to 90° C. at a rate of 2° C. / s.
[0070] The step A comprises the following steps: after the solution is cooled naturally, the solution is filtered with a 0.1 micron microporous filter membrane, the product is repeatedly washed with deionized water until the filtrate is neutral, dried in a vacuum oven at 40° C. for 24 hours, and ground and sieved with a mortar after the solution is cooled naturally.
[0071] In the step S4, the obtained membrane electrode is placed in a vacuum oven at 40° C. and dried for 4 hours to completely evaporate the dispersed solvent in the anode and cathode catalyst layers to prepare the ordered membrane electrode.
[0072] The membrane electrode prepared in Example 3 is compared with the membrane electrode prepared by the conventional method:
[0073] Comparative Example 1:
[0074] The membrane electrode prepared using the technical content of the patent document A proton exchange membrane fuel cell membrane electrode catalyst layer and its preparation method, application number: 202311679924.4:
[0075] Weigh 20 g of Pt / C catalyst and place it in a beaker, add 80 mL of ultrapure water, 80 mL of isopropanol and 40 g of Nafion resin mixed solution (D2020), mix and disperse first, then high-pressure homogenize and disperse at 20000 psi, and finally stir and disperse thoroughly to form a catalyst ink; then use a slit coating method to apply the ink to the front and back surfaces of a proton exchange membrane with an area of 130 mm*280 mm, and dry it to obtain a proton exchange membrane fuel cell membrane electrode catalyst layer.
[0076] The present invention solves the problem that the proton transport on the cathode side of the membrane electrode of the proton exchange membrane fuel cell prepared by the traditional method is seriously dependent on the intrinsic dispersion characteristics of the ionomer in the slurry, the continuity of the constructed proton transport skeleton network is poor, and the proton conductivity is low. Figure 4 As shown, the cathode side proton impedance was measured by the hydrogen pump method and it was found that the cathode side proton impedance of the membrane electrode prepared by the present invention was reduced by more than 47% compared with the membrane electrode prepared by the traditional method.
[0077] The present invention solves the problem that the electron transport on the cathode side of the membrane electrode of the proton exchange membrane fuel cell prepared by the traditional method is seriously dependent on the intrinsic dispersion characteristics of the catalyst agglomerates in the slurry, the continuity of the constructed electron transport skeleton network is poor, and the electron conductivity is low. Figure 5 As shown, the cathode side electron transfer impedance was measured by AC impedance spectroscopy and it was found that the cathode side proton impedance of the membrane electrode prepared by the present invention was reduced by more than 34% compared with the membrane electrode prepared by the traditional method.
[0078] The present invention solves the problem of low utilization rate of precious metal catalysts on the cathode side of the membrane electrode of a proton exchange membrane fuel cell prepared by a conventional method at low loading due to poor continuity of the proton transmission channel and poor continuity of the electron transmission channel. Figure 6 As shown, under the three conditions of low platinum loading, medium platinum loading and high platinum loading, the effective electrochemical active area on the cathode side of the membrane electrode prepared by this method is higher than that of the membrane electrode prepared by the traditional method.
[0079] The present invention greatly simplifies the preparation process of ordered proton exchange membrane fuel cell membrane electrode, and can achieve ultra-high performance at low loading. Figure 7 As shown, at the same low platinum loading level on the cathode side, the peak power of the membrane electrode prepared by the present invention is 37% higher than that of the membrane electrode prepared by the traditional method.
Claims
1. A method for preparing a fuel cell membrane electrode, characterized in that: The following steps are involved: S1: Mix carbon nanotubes and sulfuric acid, stir and heat the solution, add NaMnO4 and continue stirring, inject water after stirring, add hydrogen peroxide solution, wash the obtained product with water, centrifuge, precipitate and dry to obtain solid A; S2: loading platinum particles onto the surface of solid A to obtain catalyst B; S3: diluting the PFSA ionomer solution with isopropanol to obtain solution C, placing catalyst B in solution C, stirring, centrifuging and washing the product repeatedly until the supernatant is clear, and drying to obtain product solid particles D, then placing solid particles D in solution C and stirring, centrifuging, washing, and drying the product to obtain solid particles E; S4: The solid particles E are mixed with water and isopropanol, and after ultrasonic treatment, a slurry is obtained. The slurry is sprayed as cathode slurry on the other side of the proton exchange membrane on the prepared anode side to obtain a membrane electrode, and finally dried.
2. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: In the step S1, the carbon nanotubes and sulfuric acid with a concentration of 0.5-1.5M are mixed, the rotor speed is adjusted to 1200rpm at room temperature, and the mixture is stirred at a constant speed for 12-36h until a homogeneous black viscous solution is formed; NaMnO4 is slowly added during the heating process until the heating is completed, and the stirring is continued for 12-36h. After the stirring is completed, deionized water is injected, and then a hydrogen peroxide solution with a mass concentration of 2-6% is added. During the liquid preparation process, the rotor speed is adjusted to 1200rpm, and stirring is maintained. After the reaction is complete, the solution is allowed to stand for 12 hours, and the obtained product is repeatedly washed with deionized water, centrifuged, precipitated, and dried after the supernatant is clarified.
3. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: In the step S2, after a 40-60% mass concentration of formaldehyde solution and a chloroplatinic acid solution are mixed with solid A, deionized water is added and stirred for 10-50 minutes, ultrasonicated for 0.5-3 hours, condensed and refluxed in an oil bath environment of 100-140° C. for 2-8 hours, left for 10-20 hours to allow the solution to cool naturally, and treated by step A to obtain catalyst B; step A comprises the following steps: after the solution is naturally cooled, suction filtered with a 0.1 micron microporous filter membrane, repeatedly washing the product with deionized water until the filtrate is neutral, drying in a vacuum oven at 30-60° C. for 18-30 hours, and grinding and sieving after natural cooling.
4. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: In the step S3, the PFSA ionomer solution with an initial mass concentration of 20% is diluted with isopropanol to a mass concentration of 0.15-0.35% to obtain a solution C, the catalyst B is placed in the solution C, and magnetically stirred for 20-40 hours, the product is repeatedly centrifuged and washed until the supernatant is clear, and dried to obtain a product solid particle D, and then the solid particle D is placed in the diluted solution C and magnetically stirred for 20-40 hours, the product is repeatedly centrifuged and washed until the supernatant is clear, and dried to obtain a product solid particle E.
5. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: In the step S4, the obtained solid particles E are mixed with deionized water and isopropanol in a mass ratio of 1:10-40:100-300, ultrasonicated for 5-20 hours, and then sprayed.
6. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: In the step S1, after stirring, the solution is heated to 70-110° C. at a rate of 1-5° C. / s.
7. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: In the step S4, the obtained membrane electrode is placed in a vacuum oven at 30-60° C. and dried for not less than 3 hours.
8. A membrane electrode prepared by the method according to any one of claims 1 to 7.
9. A fuel cell made using the membrane electrode according to claim 8.
Citation Information
Patent Citations
Ordered membrane electrode of proton-exchange membrane fuel battery, preparation and application thereof
CN100517820C
Method for preparing nitrogen-doped carbon nanotube fuel cell catalyst
CN102416337A
Nano-fiber catalyst layer membrane based on electrostatic spinning, fuel cell membrane electrode and preparation method of nano-fiber catalyst layer membrane and fuel cell membrane electrode
CN116093345A
Membrane electrode catalyst layer of proton exchange membrane fuel cell and preparation method of membrane electrode catalyst layer
CN117673386A
Phosphoric-acid-functionalized carbon nano tubes (CNTs)-supported Pt catalyst for direct methanol fuel cell and preparation method of catalyst
CN105056942A