A marine liquefied natural gas fuel decarbonization catalyst

By using a molten catalyst composed of sodium chloride, copper chloride, and nickel chloride, the problem of high catalyst cost in LNG fuel ship decarbonization technology has been solved, achieving efficient CH4 conversion and low emissions.

CN118616061BActive Publication Date: 2026-11-17SOUTHWEST PETROLEUM UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410657493.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-25
Publication Date
2026-11-17
Estimated Expiration
2044-05-25

AI Technical Summary

Technical Problem

In existing decarbonization technologies for LNG-fueled ships, molten metal catalysts are expensive and require large filling volumes, resulting in excessively high usage costs and making them difficult to promote.

Method used

A molten catalyst composed of sodium chloride, copper chloride, and nickel chloride, with an optimal molar ratio of 12.7:1:1, is used for catalytic cracking of liquefied natural gas, forming a loose and porous structure, reducing the amount of catalyst required, and improving activity.

Benefits of technology

At 950℃, the CH4 conversion rate reaches 60%, the hydrogen concentration reaches 75%, and the CO2 emission per kilojoule of heat is reduced to 12.8 ml, thus reducing the cost of catalyst use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118616061B_ABST
    Figure CN118616061B_ABST
Patent Text Reader

Abstract

This invention discloses a decarbonization catalyst for marine liquefied natural gas fuel, belonging to the field of marine power equipment. It comprises the following components in molten state with the following molar ratios: sodium chloride: 11-13 parts; copper chloride: 0-1.5 parts; nickel chloride: 0-1.5 parts. In the initial stage of the reaction, NiCl2 and CuCl2 in the melt act as reactive substances, catalyzing the cracking of CH4 to produce hydrogen and carbon. This process does not consume the two metal salts. Subsequently, the H2 in the product can further react with NiCl2 and CuCl2, reducing them to solid metals Ni and Cu. The reduced metal atoms, under the action of bubbles and molten salt, grow into a loose porous structure. Under these conditions, the methane catalytic cracking activity of the system will further increase, and the molten salt can be evenly distributed within it, constantly scouring the carbon products on the surface, avoiding carbon accumulation on the metal surface, thus exhibiting excellent stability. The conversion rate can reach 60%, and the hydrogen concentration in the converted fuel gas can reach 75%. Direct combustion provides energy, with approximately 12.8 ml of CO2 emitted per kilojoule of heat. The catalyst dosage is low, resulting in low operating costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of marine propulsion systems, and in particular to a marine liquefied natural gas fuel decarbonization catalyst. Background Technology

[0002] As environmental issues become increasingly serious, carbon emissions have become a growing concern across all industries. Currently, for shipping, new energy sources, primarily LNG, are becoming a development trend. However, LNG-powered ships can only achieve approximately 20% carbon emission reduction at present, making the development of decarbonization technology for LNG fuel crucial.

[0003] Currently, the most common method for LNG decarbonization is cracking to produce hydrogen. This method achieves low carbon emissions and low cost, and the process does not produce CO2. X It is a byproduct and can generate valuable carbon products such as carbon black, carbon nanotubes, and carbon nanofibers, so it is currently widely used. Since methane has a highly stable tetrahedral structure (CH4), the breaking of its CH bonds requires a high activation energy. Therefore, catalysts play a significant role in the cracking process. Currently, molten metal catalysts are the most common. However, these catalysts have a high molten density, resulting in high catalyst filling costs. They require a large amount of catalyst and place high demands on the load-bearing capacity of the reaction device, greatly increasing the cost of use and hindering its widespread adoption. Summary of the Invention

[0004] To address the above problems, this invention provides a marine liquefied natural gas fuel decarbonization catalyst, which has the advantages of high catalytic efficiency, low dosage, and low operating cost.

[0005] The technical solution of this invention is:

[0006] A marine liquefied natural gas fuel decarbonization catalyst comprises the following components in molar proportions:

[0007] Sodium chloride: 11-13 parts;

[0008] Copper chloride: 0-1.5 parts;

[0009] Nickel chloride: 0-1.5 parts.

[0010] The catalyst is in a molten state when not in use.

[0011] The optimal reaction temperature for the catalyst is 850℃~950℃.

[0012] The optimal molar ratio of the catalyst is: sodium chloride: 12.7 parts; copper chloride: 1 part; nickel chloride: 1 part.

[0013] The beneficial effects of this invention are:

[0014] The molten salt catalyst designed in this invention can achieve a conversion rate of 60% under pure CH4 conditions at 950℃, and the hydrogen concentration in the converted fuel gas can reach 75%. It can be directly combusted for energy, and emits about 12.8 ml of CO2 per kilojoule of heat. The catalyst dosage is small and the cost of use is low. Attached Figure Description

[0015] Figure 1 This is the trend of catalytic cracking performance of the catalyst described in the embodiments of the present invention as a function of CH4 introduction time, tested under the conditions of 950°C, 20% CH4, and total inlet flow rate of 100 sccm.

[0016] Figure 2 This describes the change in H2 concentration in the product as a function of CH4 introduction time, obtained by testing the catalyst described in this embodiment of the invention under the conditions of 950°C, 20% CH4, and a total inlet flow rate of 100 sccm. Detailed Implementation

[0017] The embodiments of the present invention will be further described below with reference to the accompanying drawings.

[0018] This technology uses molten sodium chloride as the reaction molten environment, with a certain proportion of NiCl2 and CuCl2 salts added as active catalysts for the cracking reaction. In the initial stage of the reaction, NiCl2 and CuCl2 in the melt act as reactive substances, catalyzing the cracking of CH4 to produce hydrogen and carbon. This process does not consume the two metal salts. Subsequently, the H2 in the product can further react with NiCl2 and CuCl2, reducing it to solid metals Ni and Cu. The reduced metal atoms, under the action of bubbles and molten salt, grow into a loose, porous structure. Under these conditions, the methane catalytic cracking activity of the system will further increase, and the molten salt can be uniformly distributed within it, constantly scouring the surface carbon products and preventing carbon accumulation on the metal surface, thus exhibiting excellent stability.

[0019] Example 1:

[0020] A marine liquefied natural gas (LNG) fuel decarbonization catalyst was developed. First, the volume of the reactor heating zone was measured to determine the total amount (M) of the molten salt catalyst required. In this embodiment, the heating zone of the reaction tube had dimensions of Ф15mm × 300mm, and the total amount (M) was 70g. Then, the mass of the three salts was calculated based on the molar ratio of NaCl:NiCl2:CuCl2 = 12.7:1:1. Since all three salts have a certain degree of hygroscopicity, after weighing, they needed to be thoroughly mixed and ground before being filled into the reaction tube and placed in a heating furnace for dehydration. The dehydration temperature was set at 150℃, and the dehydration time was 1 hour. During dehydration, 80 sccm of Ar gas was introduced to accelerate the outflow of water vapor. After dehydration, the temperature was raised to 950℃ for catalyst pretreatment. Once the reactor temperature stabilized at 950℃, 20% CH4 gas was introduced, and the reaction tail gas was passed through a chromatograph to monitor the CH4 concentration in real time. The results showed that at 950℃, the catalyst basically completed the phase change after 140 minutes of CH4 gas introduction in this stage. The conversion rate of CH4 and the hydrogen yield of the melt gradually increased. After 5 hours of reaction, the CH4 conversion rate reached 80% and the H2 concentration in the tail gas reached 30%.

[0021] Example 2:

[0022] Under the same conditions as in Example 1, the molar ratio of the three salts NaCl:NiCl2:CuCl2 was changed to 25.4:1:2. The results showed that at 950°C, the catalyst pretreatment was basically completed after 100 minutes of CH4 gas introduction. The conversion rate of CH4 and the hydrogen yield of the melt gradually increased, but the rate of increase was significantly slower than in Example 1. After 5 hours of reaction, the CH4 conversion rate reached 37.4%, and the H2 concentration in the tail gas reached 14.9%.

[0023] Example 3:

[0024] Under the same conditions as in Example 1, NiCl2 was not used in the catalyst, and the molar ratio of the other two salts was NaCl:CuCl2 = 12.7:1. The results showed that under these conditions, the conversion rate of CH4 in the system was stable at around 13%, which was nearly 70% lower than that in Example 1.

[0025] Example 4:

[0026] Under the same conditions as in Example 1, CuCl2 was not used in the catalyst, and the molar ratio of the other two salts was NaCl:NiCl2 = 12.7:1. The results showed that under these conditions, the conversion rate of CH4 in the system also showed a trend of first decreasing, then increasing, and finally stabilizing. However, compared with Example 1, the decrease in conversion rate in the early stage of the reaction was smaller. After 3 hours of reaction, the conversion rate began to increase, but the increase was slow and the increase was small. It is expected that the conversion rate will remain at around 38% after stabilizing.

[0027] The overall results show that direct combustion of LNG fuel for energy produces approximately 25.2 ml of CO2 emissions per kilojoule of heat; Figure 1 , Figure 2 As shown, if the molten salt catalyst designed in this invention can achieve a conversion rate of 60% under pure CH4 conditions at 950℃, the hydrogen concentration in the converted fuel gas can reach 75%, and it can be directly burned for energy, with CO2 emissions of approximately 12.8 ml per kilojoule of heat.

[0028] The embodiments described above are merely illustrative of specific implementations of the present invention, and while the descriptions are detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention.

Claims

1. A marine liquefied natural gas fuel decarburization catalyst characterized by, The catalyst comprises the following components in the following molar ratios: Sodium chloride: 12.7 parts; Copper chloride: 1 part; Nickel chloride: 1 part; The optimal reaction temperature of the catalyst is 950°C; The catalyst is in a molten state when not in use.

Citation Information

Patent Citations

  • Preparation method and application of metal-molten salt for producing hydrogen and carbon black from natural gas

    CN114804023A

  • Pyrolysis of methane with a molten salt based catalyst system

    US20210363013A1