A methanol steam reforming hydrogen production catalyst and its preparation method, and a methanol steam reforming hydrogen production method thereof.
By preparing an MCM-41 support and loading it with active metal components, the problem of catalyst sintering at high temperatures was solved, enabling a highly efficient methanol steam reforming process for hydrogen production. This improved the catalyst's activity and lifespan while reducing preparation and operating costs.
Patent Information
- Application Number
- CN202410666720.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-28
AI Technical Summary
Existing methanol steam reforming catalysts for hydrogen production are prone to sintering at high temperatures, leading to loss of active sites and a decrease in specific surface area, resulting in reduced catalytic activity and service life.
MCM-41 support was prepared by hydrothermal crystallization using a mixture of template agent aqueous solution and silicon source. The active metal component was loaded and formed uniformly dispersed active sites by grinding and calcining the homogeneous template agent, which in turn enhanced the catalytic activity in conjunction with the auxiliary component.
The prepared catalyst exhibits excellent catalytic activity and stability, reduces preparation complexity, shortens hydrogen reduction processing time, and lowers the cost of methanol-to-hydrogen production.
Smart Images

Figure CN118616084B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalytic materials technology, specifically relating to a methanol steam reforming hydrogen production catalyst and its preparation method, as well as a methanol steam reforming hydrogen production method. Background Technology
[0002] With population growth and the expansion of energy-intensive industries, the demand for energy is gradually increasing. Traditional fossil fuel energy systems are a major source of greenhouse gas emissions. Hydrogen energy, a green energy source, is a very promising alternative to fossil fuels and can be used as an energy storage material in many systems, with broad application prospects. Methanol, as an important chemical, can react with water to release three times its volume of hydrogen. Its good balance between high hydrogen storage capacity and mild hydrogen production conditions makes it an important hydrogen energy carrier.
[0003] The methanol steam reforming process for hydrogen production generally requires the use of a catalyst to ensure stable and efficient reaction. Currently used catalysts for methanol steam reforming for hydrogen production are mainly copper-zinc-aluminum catalysts. These catalysts are usually prepared using the traditional co-precipitation method, which is relatively complex. Furthermore, sintering at 300℃ can easily lead to the loss of active sites and a decrease in specific surface area, thereby reducing the catalytic activity and lifespan of the catalyst. Summary of the Invention
[0004] The purpose of this invention is to provide a methanol steam reforming hydrogen production catalyst and its preparation method, as well as a methanol steam reforming hydrogen production method. The preparation method of the methanol steam reforming hydrogen production catalyst of this invention is simple, the reaction conditions are mild, and the prepared catalyst has excellent catalytic activity.
[0005] To achieve the objectives of this invention, the following technical solutions are provided:
[0006] A method for preparing a methanol steam reforming catalyst for hydrogen production includes the following steps:
[0007] The template agent aqueous solution and silicon source were mixed and subjected to hydrothermal crystallization, followed by solid-liquid separation to obtain the MCM-41 carrier;
[0008] The metal solid solution and the MCM-41 support are ground with a homogeneous template agent to obtain a precursor; the metal solid solution includes an active metal salt and an auxiliary metal salt; the metal in the active metal salt is one or more of Cu, Zn and Ni; the metal in the auxiliary metal salt is one or more of Ce, Zr, Mg and Al.
[0009] The precursor is calcined to obtain the methanol steam reforming hydrogen production catalyst.
[0010] Preferably, the template agent in the aqueous template solution is hexadecyltrimethylammonium bromide or hexadecyltrimethyl-p-toluenesulfonium; the concentration of the aqueous template agent solution is 1-8 wt%.
[0011] Preferably, the silicon source includes one of methyl orthosilicate, ethyl orthosilicate, and silica sol.
[0012] Preferably, the mass ratio of template agent to silicon source in the template agent aqueous solution is 0.5-4:6-10; the mass ratio of carrier MCM-41, active metal salt and auxiliary metal salt is 1:0.05-0.2:0.02-0.08.
[0013] Preferably, the hydrothermal crystallization temperature is 80–140°C and the time is 30–60 h.
[0014] Preferably, the homogeneous template agent is ground at a rate of 40–100 rpm for 5–60 min.
[0015] Preferably, the roasting temperature is 350–750°C and the time is 1–9 hours.
[0016] The present invention also provides a methanol steam reforming hydrogen production catalyst prepared by the preparation method described above, comprising an MCM-41 support and an active metal component and an auxiliary metal component supported in the pores of the MCM-41 support.
[0017] This invention also provides a method for producing hydrogen by methanol steam reforming, comprising the following steps:
[0018] The methanol steam reforming hydrogen production catalyst described in the above technical solution is reduced, and then the methanol steam reforming hydrogen production reaction is carried out to obtain hydrogen.
[0019] Preferably, the reduction treatment is carried out in a hydrogen-containing atmosphere, wherein the volume fraction of hydrogen in the hydrogen-containing atmosphere is 10-20%; the temperature of the reduction treatment is 200-400℃ and the time is 0.5-2h; the temperature of the methanol steam reforming to produce hydrogen is 200-400℃ and the time is 5-12h.
[0020] This invention provides a method for preparing a methanol steam reforming hydrogen production catalyst, comprising the following steps: mixing an aqueous template agent and a silicon source, performing hydrothermal crystallization, and obtaining an MCM-41 support through solid-liquid separation; grinding a metal solid solution and the MCM-41 support with a homogeneous template agent to obtain a precursor; the metal solid solution comprises an active metal salt and an auxiliary metal salt; the active metal salt comprises one or more of Cu, Zn, and Ni; the auxiliary metal salt comprises one or more of Ce, Zr, Mg, and Al; and calcining the precursor to obtain the methanol steam reforming hydrogen production catalyst. The method for preparing the methanol steam reforming hydrogen production catalyst provided by this invention is simple to operate, has mild reaction conditions, reduces the complexity of preparation, and is suitable for large-scale production. This invention employs a homogeneous template grinding method, which ensures that the template occupies most of the space in the pores of the MCM-41 support during subsequent calcination. This allows the active metal particles to disperse between the template and the silicon wall (SiO2 structure of MCM-41) of the MCM-41 support. This dispersion method effectively inhibits the aggregation of active components, resulting in a large number of uniformly dispersed active sites on the catalyst. This effectively achieves uniform loading of active components and, in conjunction with the auxiliary components, further enhances the catalytic activity and selectivity of the catalyst.
[0021] The present invention also provides a method for producing hydrogen from methanol by steam reforming. The method uses the methanol steam reforming hydrogen production catalyst described in the present invention to improve the catalytic activity of the catalyst, shorten the time of hydrogen reduction treatment in practical applications, and reduce the cost of methanol to hydrogen production. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 XRD pattern of the MCM-41 catalyst prepared for the test example;
[0024] Figure 2 BET plot of the MCM-41 catalyst prepared for the test example;
[0025] Figure 3 The pore size distribution of the MCM-41 catalyst prepared for the test example is shown in the diagram.
[0026] Figure 4 TEM image of the MCM-41 catalyst prepared for the test example;
[0027] Figure 5The XRD pattern of the CuZr / MCM-41 catalyst prepared in Example 2;
[0028] Figure 6 The BET plot shows the CuZr / MCM-41 catalyst prepared in Example 2.
[0029] Figure 7 The pore size distribution diagram is shown for the CuZr / MCM-41 catalyst prepared in Example 2.
[0030] Figure 8 This is a TEM image of the CuZr / MCM-41 catalyst prepared in Example 2. Detailed Implementation
[0031] This invention provides a method for preparing a methanol steam reforming catalyst for hydrogen production, comprising the following steps:
[0032] The template agent aqueous solution and silicon source were mixed and subjected to hydrothermal crystallization, followed by solid-liquid separation to obtain the MCM-41 carrier;
[0033] The metal solid solution and the MCM-41 support are ground with a homogeneous template agent to obtain a precursor; the metal solid solution includes an active metal salt and an auxiliary metal salt; the metal in the active metal salt is one or more of Cu, Zn and Ni; the metal in the auxiliary metal salt is one or more of Ce, Zr, Mg and Al.
[0034] The precursor is calcined to obtain the methanol steam reforming hydrogen production catalyst.
[0035] In this invention, unless otherwise specified, all raw materials used in the preparation are preferably commercially available products well known to those skilled in the art.
[0036] This invention involves mixing an aqueous template agent solution and a silicon source, followed by hydrothermal crystallization, and then solid-liquid separation to obtain the MCM-41 carrier. In this invention, the template agent in the aqueous template agent solution is preferably hexadecyltrimethylammonium bromide or hexadecyltrimethyl-p-toluenesulfonium; the concentration of the aqueous template agent solution is preferably 1–8 wt%, more preferably 2–7 wt%, and even more preferably 3–5 wt%. In this invention, the pH value of the aqueous template agent solution is preferably adjusted before use; the reagent for adjusting the pH value is preferably ammonia; the concentration of the ammonia is preferably 20–30 wt%; and the pH value of the aqueous template agent solution is preferably 8–12, more preferably 9–11.
[0037] In this invention, the silicon source preferably includes one of methyl orthosilicate, tetraethyl orthosilicate, and silica sol, more preferably tetraethyl orthosilicate.
[0038] In this invention, the mass ratio of template agent to silicon source in the template agent aqueous solution is preferably 0.5-4:6-10, more preferably 1-3:7-9.
[0039] In this invention, the mixing of the template agent aqueous solution and the silicon source is preferably carried out under stirring conditions. Preferably, the silicon source is added dropwise to the template agent aqueous solution to obtain a suspension. In this invention, the dropping rate of the silicon source is preferably 2–10 d / min, more preferably 3–8 d / min; the mixing time is preferably 6–24 h, more preferably 8–12 h. This invention enhances the structural order of the carrier MCM-41 by adding the silicon source dropwise.
[0040] In this invention, the hydrothermal crystallization temperature is preferably 80–140°C, more preferably 90–120°C; the time is preferably 30–60 h, more preferably 40–50 h; the hydrothermal crystallization is preferably carried out in an air atmosphere; the hydrothermal crystallization is preferably carried out in a forced-air drying oven. This invention thickens the pore walls of the prepared carrier MCM-41 through hydrothermal crystallization, thereby improving the hydrothermal stability of the carrier MCM-41.
[0041] The present invention does not have any particular limitation on the method of solid-liquid separation, and any solid-liquid separation method known to those skilled in the art can be used.
[0042] In this invention, the solid product after solid-liquid separation is preferably dried to obtain the MCM-41 carrier. The drying temperature is preferably 90–120°C, more preferably 100–110°C; the drying time is preferably 6–18 hours, more preferably 8–12 hours; and the drying is preferably carried out in a forced-air drying oven.
[0043] After obtaining the MCM-41 support, the present invention grinds the metal solid solution and the MCM-41 support using a homogeneous template agent to obtain a precursor. In the present invention, the metal in the active metal salt is one or more of Cu, Zn, and Ni, preferably Cu; the active metal salt is preferably one or more of nitrate, sulfate, hydrochloride, and acetate, more preferably nitrate. In a specific embodiment of the present invention, the active metal salt is preferably Cu(NO3)2.
[0044] In this invention, the metal in the auxiliary metal salt is one or more of Ce, Zr, Mg, and Al, preferably Zn or Zr; the auxiliary metal salt is preferably one or more of nitrate, sulfate, hydrochloride, and acetate, more preferably nitrate. In a specific embodiment of this invention, the auxiliary metal salt is preferably Zr(NO3)4 or Zn(NO3)2.
[0045] In this invention, the preferred mass ratio of the carrier MCM-41, the active metal salt, and the auxiliary metal salt is 1:0.05–0.2:0.02–0.08, more preferably 1:0.05–0.15:0.02–0.06. By controlling the mass ratio of the active metal salt, the auxiliary metal salt, and the MCM-41 carrier within the above range, this invention helps ensure a high degree of dispersion of the active metal component and the auxiliary metal component in the catalyst during subsequent calcination.
[0046] In this invention, the metal solid solution is preferably prepared by microwave impregnation or microwave precipitation. This invention does not impose any particular limitations on the conditions for microwave impregnation or microwave precipitation. This invention ensures that the active metal component and the metal additive component are thoroughly and uniformly mixed during the preparation of the metal solid solution.
[0047] In this invention, the grinding rate of the homogeneous template agent is preferably 40-80 rpm, more preferably 50-70 rpm, and the grinding time is preferably 10-60 min, more preferably 30-40 min. By controlling the grinding conditions of the homogeneous template agent within the above range, this invention enables the active metal and auxiliary metal to be uniformly dispersed within the pores of the MCM-41 carrier without damaging the pore structure of the MCM-41 carrier.
[0048] After obtaining the precursor, the present invention calcines the precursor to obtain the methanol steam reforming hydrogen production catalyst. In the present invention, the calcination temperature is preferably 350–750°C, more preferably 400–700°C; the time is preferably 1–9 h, more preferably 2–8 h; the heating rate to the calcination temperature is preferably 0.5–3°C / min, more preferably 1–2°C / min; the cooling rate after calcination is preferably 0.5–3°C / min, more preferably 1–2°C / min; the calcination apparatus is preferably a muffle furnace; and the calcination is preferably carried out under air conditions. By controlling the calcination temperature, time, and heating / cooling rates within the above ranges, the present invention can slowly remove the template agent while ensuring the ordered structure of the MCM-41, which is beneficial for the uniform distribution of active and auxiliary components within the MCM-41 channels, thereby improving the activity and selectivity of the finally prepared catalyst.
[0049] The present invention also provides a methanol steam reforming hydrogen production catalyst prepared by the preparation method described above, comprising an MCM-41 support and an active metal component and an auxiliary metal component supported in the pores of the MCM-41 support.
[0050] In this invention, the specific surface area of the methanol steam reforming hydrogen production catalyst is preferably 600-700 m². 2 / g, more preferably 641.4~680m 2 / g, with a pore volume preferably of 0.5–0.8 cm³. 3 / g, more preferably 0.662~0.70cm 3 / g, with an average pore size preferably of 3-4 nm, more preferably 3.34-3.50 nm.
[0051] In this invention, the active metal component is preferably one or more of CuO, NiO and ZnO, more preferably CuO; the auxiliary component is preferably one or more of CeO2, ZrO2, MgO and Al2O3, more preferably ZnO or ZrO2.
[0052] This invention also provides a method for producing hydrogen by methanol steam reforming, comprising the following steps:
[0053] The methanol steam reforming hydrogen production catalyst described in the above technical solution is reduced, and then the methanol steam reforming hydrogen production reaction is carried out to obtain hydrogen.
[0054] In this invention, the reduction treatment is carried out in a hydrogen-containing atmosphere, wherein the volume fraction of hydrogen in the hydrogen-containing atmosphere is preferably 10-15%; the temperature of the reduction treatment is preferably 200-400°C, more preferably 300-350°C; and the time is preferably 0.5-2h, more preferably 1-1.5h.
[0055] In this invention, the feedstock for the methanol steam reforming hydrogen production reaction is preferably an aqueous methanol solution; the molar ratio of methanol to water in the aqueous methanol solution is preferably 1:1 to 1.8, more preferably 1:1.4 to 1.6; and the influent mass hourly space velocity (MHV) of the aqueous methanol solution is preferably 1 to 6 h⁻¹. -1 More preferably 2 to 3.58h -1 The preferred influent flow rate is 0.005–0.02 mL / min, more preferably 0.01 mL / min.
[0056] In this invention, the temperature of the methanol steam reforming hydrogen production reaction is preferably 200-400°C, more preferably 280-350°C; the time is preferably 5-12 hours, more preferably 8-12 hours.
[0057] In this invention, when the flow rate of the methanol aqueous solution is preferably 0.005 to 0.02 mL / min, the amount of the catalyst is preferably 0.1 to 0.3 g, more preferably 0.15 to 0.25 g.
[0058] To further illustrate the present invention, the following detailed description, in conjunction with the accompanying drawings and embodiments, describes a methanol steam reforming hydrogen production catalyst and its preparation method, as well as a methanol steam reforming hydrogen production method, provided by the present invention. However, these descriptions should not be construed as limiting the scope of protection of the present invention.
[0059] Example 1
[0060] 2.12 g of hexadecyltrimethylammonium bromide was dissolved in 50 mL of deionized water. The pH of the resulting hexadecyltrimethylammonium bromide aqueous solution was adjusted to 11 using 11.2 g of 25 wt% ammonia solution. 8.66 g of tetraethyl orthosilicate was added dropwise at 60 rpm for 6 days / min. After mixing for 12 hours, a suspension was obtained. The suspension was placed in a reaction vessel and hydrothermally crystallized at 110 °C in air for 48 hours. Then, it was filtered, and the filter cake was dried at 100 °C for 12 hours to obtain the MCM-41 support.
[0061] Cu(NO3)2 and Zn(NO3)2 in a mass ratio of 5:2 were processed into a metal solid solution by microwave impregnation; 0.04 g of the above metal solid solution and 0.2 g of the above MCM-41 support were ground with a homogeneous template agent at 60 rpm for 10 min to obtain the precursor.
[0062] The temperature was increased to 550℃ at a heating rate of 1.5℃ / min, and the precursor was calcined at 550℃ for 6 hours. Then, it was cooled to room temperature at a cooling rate of 2℃ / min to obtain the methanol steam reforming hydrogen production catalyst, denoted as CuZn / MCM-41 catalyst.
[0063] Example 2
[0064] 2.12 g of hexadecyltrimethylammonium bromide was dissolved in 50 mL of deionized water. The pH of the resulting hexadecyltrimethylammonium bromide aqueous solution was adjusted to 11 using 11.2 g of 25% ammonia solution. 8.66 g of tetraethyl orthosilicate was added dropwise at 60 rpm and 6 d / min. After mixing for 12 h, a suspension was obtained. The suspension was placed in a reaction vessel and hydrothermally crystallized at 110 °C in air for 48 h. Then, it was filtered, and the filter cake was dried at 100 °C for 12 h to obtain the MCM-41 support.
[0065] Cu(NO3)2 and Zr(NO3)4 in a mass ratio of 5:2 were processed into a metal solid solution by microwave impregnation; 0.04 g of the above metal solid solution and 0.2 g of the above MCM-41 support were ground with a homogeneous template agent at 60 rpm for 10 min to obtain the precursor.
[0066] The temperature was increased to 550℃ at a heating rate of 1.5℃ / min, and the precursor was calcined at 550℃ for 6 hours. Then, it was cooled to room temperature at a cooling rate of 2℃ / min to obtain the methanol steam reforming hydrogen production catalyst, denoted as CuZr / MCM-41 catalyst.
[0067] Test case
[0068] The MCM-41 support prepared in Example 1 was calcined at 550°C for 6 hours to obtain the MCM-41 catalyst. The specific surface area of the MCM-41 catalyst was analyzed by BET, and the pore volume and pore size of the MCM-41 catalyst were analyzed by the BJH method. The specific surface area of the prepared MCM-41 catalyst was measured to be 819.2 m². 2 / g, pore volume is 0.784cm³ 3 / g, with an average pore size of 3.03nm.
[0069] Figure 1 The XRD pattern of the MCM-41 catalyst prepared for the test example is shown below. Figure 1 It can be seen that the MCM-41 catalyst prepared by the hydrothermal-precipitation method has a highly ordered structure.
[0070] Figure 2 The BET plot shows the MCM-41 catalyst prepared for the test example. Figure 3 The pore size distribution diagram of the MCM-41 catalyst prepared for the test example is shown below. Figures 2-3 It can be seen that the MCM-41 catalyst prepared by the hydrothermal-precipitation method is a mesoporous material with uniform cylindrical channels.
[0071] Figure 4 TEM image of the MCM-41 catalyst prepared for the test example, by Figure 4 It can be seen that the MCM-41 catalyst prepared by the hydrothermal-precipitation method has a hexagonal ordered crystalline structure.
[0072] The specific surface area of the CuZr / MCM-41 catalyst prepared in Example 2 was analyzed using BET, and the pore volume and pore size of the material were analyzed using the BJH method. The specific surface area of the prepared CuZr / MCM-41 catalyst was found to be 641.4 m². 2 / g, pore volume is 0.662cm³ 3 / g, with an average pore size of 3.34nm.
[0073] Figure 5 The image shows the XRD pattern of the CuZr / MCM-41 catalyst prepared in Example 2. Figure 5 It can be seen that the CuZr / MCM-41 catalyst prepared by the homogeneous template grinding method did not destroy the highly ordered structure of MCM-41.
[0074] Figure 6 The above is a BET plot of the CuZr / MCM-41 catalyst prepared in Example 2. Figure 7 The pore size distribution diagram is shown for the CuZr / MCM-41 catalyst prepared in Example 2. Figures 6-7It can be seen that the CuZr / MCM-41 catalyst prepared by the homogeneous template grinding method still maintains the cylindrical ordered pore structure.
[0075] Figure 8 This is a TEM image of the CuZr / MCM-41 catalyst prepared in Example 2. Figure 8 It can be seen that the CuZr / MCM-41 catalyst prepared by homogeneous template grinding method has a large number of uniformly dispersed CuO active sites in the MCM-41 channels.
[0076] Application Example 1
[0077] 0.15 g of the CuZn / MCM-41 methanol steam reforming hydrogen production catalyst prepared in Example 1 was placed in the middle of the reaction tube and subjected to reduction treatment at 300°C under a 10% hydrogen atmosphere for 1 h. Then, a methanol-water aqueous solution with a methanol-water molar ratio of 1:1.4 was pumped into the feed inlet using a feed pump at a flow rate of 0.01 mL / min and a liquid hourly space velocity (LHSV) of 3.58 h⁻¹. -1 After stable injection, methanol steam reforming to produce hydrogen was carried out at a reaction temperature of 280℃. Gas samples were collected at the reaction gas outlet, and the composition of the product gas was analyzed by gas chromatography. The results are shown in Table 1.
[0078] Application Example 2
[0079] 0.15 g of the CuZr / MCM-41 methanol steam reforming hydrogen production catalyst prepared in Example 2 was placed in the middle of the reaction tube and reduced at 300°C under a 10% hydrogen atmosphere for 1 h. Then, a methanol-water aqueous solution with a methanol-water molar ratio of 1:1.4 was pumped into the feed inlet at a flow rate of 0.01 mL / min and a liquid hourly space velocity (LHSV) of 3.58 h⁻¹. -1 After stable injection, methanol steam reforming to produce hydrogen was carried out at a reaction temperature of 280℃. Gas samples were collected at the reaction gas outlet, and the composition of the product gas was analyzed by gas chromatography. The results are shown in Table 1.
[0080] Table 1. Results Analysis of Methanol-Steam Reforming Hydrogen Production Method
[0081]
[0082] From Table 1 and Figures 5-8 It is known that the MCM-41 with high specific surface area and ordered channels prepared by the present invention effectively improves the dispersion of metal active components and auxiliary components, thereby improving the reaction activity and selectivity of the catalyst, and thus shortening the time of hydrogen reduction treatment in practical applications and reducing the cost of methanol to hydrogen production.
[0083] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. People can obtain other embodiments based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for producing a catalyst for hydrogen production by methanol steam reforming, characterized by, The steps are as follows: The template agent aqueous solution and silicon source are mixed and subjected to hydrothermal crystallization. After solid-liquid separation, the solid product after solid-liquid separation is dried to obtain the MCM-41 carrier. The drying temperature is 90~120℃. The metal solid solution and the MCM-41 support are ground with a homogeneous template agent to obtain a precursor; the metal solid solution includes an active metal salt and an auxiliary metal salt; the metal in the active metal salt is one or more of Cu, Zn and Ni; the metal in the auxiliary metal salt is one or more of Ce, Zr, Mg and Al. The precursor is calcined to obtain the methanol steam reforming hydrogen production catalyst.
2. The preparation method according to claim 1, characterized in that, The template agent in the aqueous solution is hexadecyltrimethylammonium bromide or hexadecyltrimethyl-p-toluenesulfonium; the concentration of the aqueous solution of the template agent is 1-8 wt%.
3. The preparation method according to claim 1, characterized in that, The silicon source includes one of methyl orthosilicate, ethyl orthosilicate, and silica sol.
4. The preparation method according to any one of claims 1 to 3, characterized in that, The mass ratio of template agent to silicon source in the template agent aqueous solution is 0.5~4:6~10; the mass ratio of carrier MCM-41, active metal salt and auxiliary metal salt is 1:0.05~0.2:0.02~0.
08.
5. The preparation method according to claim 1, characterized in that, The hydrothermal crystallization temperature is 80~140℃, and the time is 30~60h.
6. The preparation method according to claim 1, characterized in that, The homogeneous template agent is ground at a rate of 40-100 rpm for 5-60 min.
7. The preparation method according to claim 1, characterized in that, The roasting temperature is 350~750℃, and the time is 1~9h.
8. The methanol steam reforming hydrogen production catalyst prepared by the method according to any one of claims 1 to 7, characterized in that, It includes an MCM-41 carrier and active metal components and auxiliary metal components loaded in the pores of the MCM-41 carrier.
9. A method for producing hydrogen by methanol steam reforming, characterized in that, Includes the following steps: The methanol steam reforming hydrogen production catalyst described in claim 8 is reduced, and then a methanol steam reforming hydrogen production reaction is carried out to obtain hydrogen.
10. The method for producing hydrogen from methanol via steam reforming according to claim 9, characterized in that, The reduction process is carried out in a hydrogen-containing atmosphere, wherein the volume fraction of hydrogen in the hydrogen-containing atmosphere is 10-15%; the temperature of the reduction process is 200-400℃ and the time is 0.5-2h; the temperature of the methanol steam reforming to produce hydrogen is 200-400℃ and the time is 5-12h.
Citation Information
Patent Citations
Catalyst for hydrogen production through methanol-water vapor reforming, and preparation method thereof
CN110508315A
Copper-based catalyst for hydrogen production by methanol steam reforming and preparation method and application thereof