A method for preparing high-rate graphite negative electrode material

By using raw materials such as waste graphite electrodes, needle coke, mesophase carbon microspheres, and BFBAEPY-COF self-aggregating ligands, and through modification and granulation processes, the bottleneck problems of graphite anode material rate and cycle life performance were solved, and achieved Preparation of graphite anode materials with high rate, long life and efficient energy storage.

CN118619266BActive Publication Date: 2024-10-15WAN XIN LIAONING TECH MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411089725.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-15
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Existing graphite anode materials have bottlenecks in improving rate, cycle life and capacity performance. In particular, the rate performance is difficult to break through, and the product quality is unstable and the applicable environment is limited.

Method used

Using waste graphite electrodes, needle coke, mesophase carbon microspheres, BFBAEPY-COF self-aggregating ligands and spinning pitch as raw materials, through ball milling, pitch modification and briquetting and granulation, the material structure and performance are improved, and the rate is increased. , cycle life and energy storage capacity.

Benefits of technology

The preparation of high-rate graphite anode materials has been achieved, which improves the material's charge and discharge speed, cyclicity and environmental adaptability, reduces costs and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a preparation method of a high-rate graphite negative electrode material, which belongs to the field of new energy batteries. The preparation method adopts waste graphite electrodes, needle coke, mesophase carbon microspheres, BFBAEPY-COF self-polymerized ligands and spinning pitch as raw materials; the BFBAEPY-COF self-polymerized ligands are embedded in the needle coke through ball milling and asphalt modification, so as to improve energy storage and rate performance, and improve cyclability; the graphite electrodes, mesophase carbon microspheres and spinning pitch are subjected to briquetting and granulation treatment, so as to improve the structural property of the material, achieve good combination, improve the capacity, rate and cycle life of the material, give full play to the comprehensive advantages of the material, and take into account the improvement of performances such as energy storage capacity, charge and discharge speed and cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new energy, and specifically relates to a method for preparing a high-rate graphite negative electrode material. Background Art

[0002] In recent years, with the continuous development of the new energy vehicle industry, society has put forward higher requirements for new energy vehicles, especially in terms of endurance and safety. However, if new energy vehicles want to improve product quality and accelerate technological breakthroughs, they are mainly limited to the development of power batteries. During the use of new energy vehicle power batteries, there are problems such as high battery prices, long charging time, short mileage, poor environmental versatility, and short service life.

[0003] As the use of batteries in power vehicles continues to increase, lithium-ion batteries for power vehicles have placed more stringent performance requirements on their negative electrode materials, such as high safety performance, high rate discharge, long cycle life, and good environmental compatibility.

[0004] The negative electrode material of power lithium-ion batteries is a key factor in energy storage and endurance. Among them, artificial graphite has good comprehensive performance and outstanding advantages, and will be more widely used in power batteries and energy storage batteries. Artificial graphite has become the preferred material for negative electrode materials of lithium-ion batteries due to its low price and good safety.

[0005] However, in the market, the quality of artificial graphite varies greatly due to different raw material sources and production processes; and some performance indicators have bottlenecks that restrict each other. For example, when a battery is suitable for operation in a high-temperature environment, its performance in a low-temperature environment is limited; when a battery focuses on high specific capacity, its charging rate speed and cycle life will be affected. Summary of the invention

[0006] The problem that the capacity, rate and cycle life of existing graphite negative electrode materials are difficult to significantly improve as a whole, especially the problem that the rate performance of existing graphite negative electrode materials has always been difficult to break through. The present invention provides a method for preparing a high-rate graphite negative electrode material, using waste graphite electrodes, needle coke, mesophase carbon microspheres, BFBAEPY-COF self-polymerized ligands, and spinning asphalt as raw materials; embedding the BFBAEPY-COF self-polymerized ligands into needle coke through ball milling and asphalt modification to improve energy storage and rate performance, and improve cyclability; briquetting and granulation of graphite electrodes, mesophase carbon microspheres and spinning asphalt to improve the structural properties of the material, achieve good bonding, improve the capacity, rate, and cycle life of the material, give full play to the comprehensive advantages of the material, and take into account the improvement of energy storage capacity, charge and discharge speed, cycle life and other performance. The specific technical scheme is as follows:

[0007] A method for preparing a high-rate graphite negative electrode material comprises the following steps:

[0008] S1: waste graphite electrode as raw material A, needle coke as raw material B, homogeneous nucleated mesocarbon microspheres as raw material C, BFBAEPY-COF self-polymerized ligand as raw material D, spinning pitch as raw material E;

[0009] The median particle size D50 of raw material A is 10 μm to 16 μm; the particle size of raw material B is nanometer-level, less than 50 nm; the median particle size D50 of raw material C is 5 μm to 10 μm; the median particle size D50 of raw material D is 12 μm to 20 μm, and the median particle size D50 of raw material E is less than 1 μm;

[0010] S2: According to the mass ratio of raw material D: raw material B: raw material E = (100-120): (6-15): (1.5-3), raw material D, raw material B and raw material E are mixed by airflow to obtain a mixed material F, the mixed material F is placed in a reactor, modified at 300°C-400°C, cooled to obtain a coated modified material G, and the coated modified material G is heat-treated at 650°C-800°C to obtain a coated carbonized material H;

[0011] S3: Raw materials A, C and E are mixed according to the mass ratio of raw material A: raw material C: raw material E = (100-120): (30-40): (8-12) to obtain a mixture I, and the mixture I is dry-milled for 30-40 minutes to obtain a ball-milled material J; the ball-milled material J is briquette-formed to obtain a block material K, each block being a cube with a side length of 10 cm to 20 cm; each block of the block material K is wrapped with graphite paper, and then heat-treated at 1200°C to 1400°C. After cooling, the graphite paper is removed, and the granulated material L is obtained after crushing and classification;

[0012] S4: According to the mass ratio, granulated material L: coated carbonized material H: raw material C = (100-120): (25-35): (6-10), the granulated material L, coated carbonized material H and raw material C are mixed evenly, passed through a 300-325 mesh sieve, and the sieve under is taken to obtain a graphite negative electrode material.

[0013] In S1 of the above preparation method, the preparation method of raw material A is to remove the epidermis of the discarded graphite electrode, and then crush, coarsely grind, finely grind and classify in sequence to obtain raw material A; the crushing, coarsely grind and finely grind are all cutting and grinding.

[0014] In S2 of the above preparation method, the modified stirring speed is 60 r / min to 80 r / min.

[0015] In S2 of the above preparation method, the modification time is 2 h to 3 h.

[0016] In S2 of the above preparation method, the heat treatment time is 2h to 3h.

[0017] In S3 of the above preparation method, the thickness of the graphite paper is 0.5 mm to 1 mm.

[0018] In S3 of the above preparation method, the heat treatment time is 3h to 4h.

[0019] In S3 of the above preparation method, the median particle size D50 of the pulverization classification is 16 μm to 20 μm.

[0020] In S4 of the above preparation method, mixing is performed by double-cone spiral mixing.

[0021] Compared with the prior art, the method for preparing a high-rate graphite negative electrode material of the present invention has the following beneficial effects:

[0022] 1. The present invention uses waste graphite electrodes as raw materials, which can greatly reduce the cost of the main material while giving full play to its good high and low temperature performance; the graphite electrodes are mechanically cut and crushed to form more three-dimensional angular morphologies, which is beneficial to shorten the lithium ion insertion and extraction path of the material during charging and discharging, increase the charging and discharging speed, and increase the output power.

[0023] 2. The present invention uses graphite electrodes and mesophase carbon microspheres for briquetting and granulation. The median particle size D50 of the mesophase carbon microspheres is 5μm to 10μm, which is relatively small. The reasonable compounding and granulation of the two can change the morphology of the particles after granulation. Combining the characteristics of the graphite electrode and the mesophase carbon microspheres, the rate is further increased, and the capacity, efficiency and cyclability of the material can be improved.

[0024] 3. The present invention wraps the pressed block material with graphite paper, which can effectively isolate the block material from direct contact with the kiln environment, reduce the surface oxidation degree of the block material, and prevent the oxidizing components from affecting the capacitance and efficiency reduction; at the same time, it prevents the block material from oxidizing and peeling, thereby improving the yield.

[0025] 4. The present invention adopts nano-needle coke as a filler to fill the pore size of the BFBAEPY-COF self-polymerized ligand. On the one hand, the specific surface area of ​​the BFBAEPY-COF self-polymerized ligand is reduced to prevent the material from absorbing a large amount of water during slurry mixing, which causes the negative electrode sheet to shed powder and makes it impossible to make batteries. On the other hand, the nano-needle coke has good conductivity and energy storage effects after carbonization, thereby improving the rate performance, efficiency and cycle life of the material. On the other hand, after the BFBAEPY-COF self-polymerized ligand is embedded in the nano-needle coke, the particle size of the nano-needle coke powder will not affect the negative electrode material due to the addition of ultrafine powder. Agglomeration occurs, making slurry mixing difficult, and the electrode sheet sheds powder, hard spots and soft spots, which can ensure the smooth mixing and sheet making.

[0026] 5. Spinning asphalt is added to prepare coated modified material G. Spinning asphalt has hot-melt fluidity and viscosity. The coating of spinning asphalt can ensure that the BFBAEPY-COF self-polymerized ligands are more firmly embedded in the nano-needle coke and are not easy to fall off. The spinning asphalt has a protective effect on the carbonized needle coke after carbonization. When the battery is prepared later, the film-forming property of the particle surface and the electrolyte is better, which can effectively prevent the electrolyte from corroding the nano-needle coke and prevent the nano-needle coke from reacting with the electrolyte to expand, thereby preventing the BFBAEPY-COF self-polymerized ligands from disintegrating and falling off.

[0027] 6. BFBAEPY-COF self-polymerized ligands are embedded in nano-scale needle coke. After carbonization treatment, not only the conductivity is improved, but also it has good energy storage properties, thereby improving the capacity and efficiency of the material.

[0028] 7. The heat treatment temperature of each material of the present invention is relatively low. On the one hand, it can reduce the graphitization degree of the asphalt coating layer on the surface of the material to maintain the soft carbon layer structure of the coating layer and achieve the effect of rapid charging and discharging; on the other hand, it can avoid the excessive graphitization degree of the mesophase carbon microbeads and needle coke, which affects their compatibility with the electrolyte solution, hinders the diffusion of lithium ions from the surface into the interior of the carbonaceous particles, and makes it impossible for most crystals to quickly undergo lithium insertion and extraction reactions.

[0029] 8. Adding a small amount of mesophase carbon microspheres to the material of the present invention can help improve the rate performance of the material.

[0030] 9. The negative electrode material of the present invention has excellent capacity, efficiency and cyclability under the condition of 5C high rate charge and discharge. DETAILED DESCRIPTION

[0031] The present invention is further described below in conjunction with specific implementation cases, but the present invention is not limited to these embodiments.

[0032] Embodiment 1: A method for preparing a high-rate graphite negative electrode material, comprising the following steps:

[0033] S1: Used waste graphite electrode as raw material A, needle coke as raw material B, homogeneously nucleated mesophase carbon microspheres as raw material C, BFBAEPY-COF self-polymerized ligand as raw material D, and spinning pitch as raw material E; the median particle size D50 of raw material A is 14.35μm; the particle size of raw material B is nanometer-scale, with a particle size range of less than 50nm; the median particle size D50 of raw material C is 8.89μm; the median particle size D50 of raw material D is 17.54μm, and the median particle size D50 of raw material E is 675nm;

[0034] The preparation method of raw material A is to remove the epidermis of the waste graphite electrode, and then sequentially perform crushing, coarse pulverization, fine pulverization, and classification to obtain raw material A; the crushing, coarse pulverization, and fine pulverization are all cutting pulverization;

[0035] S2: According to the mass ratio of raw material D: raw material B: raw material E = 110:12:2.5, raw material D, raw material B and raw material E are mixed by air flow to obtain a mixture F, the mixture F is placed in a reactor, modified at 360°C, the stirring speed of the modification is 70r / min, the modification time is 2.5h, and cooled to obtain a coated modified material G, and the coated modified material G is heat treated at 700°C for 2.5h to obtain a coated carbonized material H;

[0036] S3: Raw materials A, C and E are mixed in a mass ratio of 110:35:10 to obtain a mixture I, and the mixture I is dry-milled for 35 min to obtain a ball-milled material J; the ball-milled material J is briquette-formed to obtain a block material K, each block being a cube with a side length of 15 cm; each block of the block material K is wrapped with a graphite paper of 0.8 mm thickness, and then heat-treated at 1300°C for 3.5 h. After cooling, the graphite paper is removed, and the granulated material L with a median particle size D50 of 18.23 μm is obtained;

[0037] S4: According to the mass ratio of granulated material L: coated carbonized material H: raw material C = 110:30:8, the granulated material L, coated carbonized material H and raw material C are evenly mixed by double cone spiral mixing, passed through a 325 mesh sieve, and the sieve under is taken to obtain a graphite negative electrode material.

[0038] Embodiment 2: A method for preparing a high-rate graphite negative electrode material, comprising the following steps:

[0039] S1: Used waste graphite electrode as raw material A, needle coke as raw material B, homogeneously nucleated mesophase carbon microspheres as raw material C, BFBAEPY-COF self-polymerized ligand as raw material D, and spinning pitch as raw material E; the median particle size D50 of raw material A is 10.00μm; the particle size of raw material B is nanometer-scale, with a particle size range of less than 50nm; the median particle size D50 of raw material C is 5.00μm; the median particle size D50 of raw material D is 13.45μm, and the median particle size D50 of raw material E is 493nm;

[0040] The preparation method of raw material A is to remove the epidermis of the waste graphite electrode, and then sequentially perform crushing, coarse pulverization, fine pulverization, and classification to obtain raw material A; the crushing, coarse pulverization, and fine pulverization are all cutting pulverization;

[0041] S2: According to the mass ratio of raw material D: raw material B: raw material E = 100: 6: 1.5, raw material D, raw material B and raw material E are mixed by airflow to obtain a mixed material F, the mixed material F is placed in a reactor, modified at 300 ° C, the stirring speed of the modification is 60r / min, the modification time is 2h, and cooled to obtain a coated modified material G, and the coated modified material G is heat treated at 650 ° C for 2h to obtain a coated carbonized material H;

[0042] S3: Raw materials A, C and E are mixed in a mass ratio of 100:30:8 to obtain a mixture I, and the mixture I is dry-milled for 30 min to obtain a ball-milled material J; the ball-milled material J is briquette-formed to obtain a block material K, each block being a cube with a side length of 10 cm; each block of the block material K is wrapped with a graphite paper of 0.5 mm thickness, and then heat-treated at 1200°C for 3 h. After cooling, the graphite paper is removed, and the granulated material L with a median particle size D50 of 16.68 μm is obtained.

[0043] S4: According to the mass ratio of granulated material L: coated carbonized material H: raw material C = 100:25:6, the granulated material L, coated carbonized material H and raw material C are evenly mixed by double cone spiral, passed through a 300 mesh sieve, and the sieve under is taken to obtain a graphite negative electrode material.

[0044] Embodiment 3: A method for preparing a high-rate graphite negative electrode material, comprising the following steps:

[0045] S1: Use waste graphite electrode as raw material A, needle coke as raw material B, homogeneously nucleated mesophase carbon microspheres as raw material C, BFBAEPY-COF self-polymerized ligand as raw material D, and spinning pitch as raw material E; the median particle size D50 of raw material A is 15.42μm; the particle size of raw material B is nanometer-scale, with a particle size range of less than 50nm; the median particle size D50 of raw material C is 7.63μm; the median particle size D50 of raw material D is 12.00μm, and the median particle size D50 of raw material E is 800nm;

[0046] The preparation method of raw material A is to remove the epidermis of the waste graphite electrode, and then sequentially perform crushing, coarse pulverization, fine pulverization, and classification to obtain raw material A; the crushing, coarse pulverization, and fine pulverization are all cutting pulverization;

[0047] S2: According to the mass ratio of raw material D: raw material B: raw material E = 105:8:2, raw material D, raw material B and raw material E are mixed by air flow to obtain a mixture F, the mixture F is placed in a reactor, modified at 350°C, the stirring speed of the modification is 65r / min, the modification time is 2h, and cooled to obtain a coated modified material G, and the coated modified material G is heat treated at 680°C for 2h to obtain a coated carbonized material H;

[0048] S3: Raw materials A, C and E are mixed in a mass ratio of 105:32:9 to obtain a mixture I, and the mixture I is dry-milled for 30 min to obtain a ball-milled material J; the ball-milled material J is briquette-formed to obtain a block material K, each block being a cube with a side length of 15 cm; each block of the block material K is wrapped with a graphite paper of 0.8 mm thickness, and then heat-treated at 1250°C for 3 h. After cooling, the graphite paper is removed, and the granulated material L with a median particle size D50 of 16.00 μm is obtained;

[0049] S4: According to the mass ratio of granulated material L: coated carbonized material H: raw material C = 105:28:7, the granulated material L, coated carbonized material H and raw material C are evenly mixed by double cone spiral, passed through a 300 mesh sieve, and the sieve under is taken to obtain a graphite negative electrode material.

[0050] Embodiment 4: A method for preparing a high-rate graphite negative electrode material, comprising the following steps:

[0051] S1: Used waste graphite electrode as raw material A, needle coke as raw material B, homogeneously nucleated mesophase carbon microspheres as raw material C, BFBAEPY-COF self-polymerized ligand as raw material D, and spinning pitch as raw material E; the median particle size D50 of raw material A is 16.00μm; the particle size of raw material B is nanometer-scale, with a particle size range of less than 50nm; the median particle size D50 of raw material C is 10.00μm; the median particle size D50 of raw material D is 16.53μm, and the median particle size D50 of raw material E is 742nm;

[0052] The preparation method of raw material A is to remove the epidermis of the waste graphite electrode, and then sequentially perform crushing, coarse pulverization, fine pulverization, and classification to obtain raw material A; the crushing, coarse pulverization, and fine pulverization are all cutting pulverization;

[0053] S2: According to the mass ratio of raw material D: raw material B: raw material E = 120:15:3, raw material D, raw material B and raw material E are mixed by airflow to obtain a mixture F, the mixture F is placed in a reactor, modified at 400°C, the stirring speed of the modification is 80r / min, the modification time is 3h, and cooled to obtain a coated modified material G, and the coated modified material G is heat treated at 800°C for 2.5h to obtain a coated carbonized material H;

[0054] S3: Raw materials A, C and E are mixed in a mass ratio of 120:40:12 to obtain a mixture I, and the mixture I is dry-milled for 40 min to obtain a ball-milled material J; the ball-milled material J is briquette-formed to obtain a block material K, each block being a cube with a side length of 20 cm; each block material K is wrapped with a graphite paper of 1 mm thickness, and then heat-treated at 1400°C for 4 h. After cooling, the graphite paper is removed, and the granulated material L with a median particle size D50 of 18.23 μm is obtained;

[0055] S4: According to the mass ratio of granulated material L: coated carbonized material H: raw material C = 120:35:10, the granulated material L, coated carbonized material H and raw material C are evenly mixed by double cone spiral mixing, passed through a 325 mesh sieve, and the sieve under is taken to obtain a graphite negative electrode material.

[0056] Embodiment 5: A method for preparing a high-rate graphite negative electrode material, comprising the following steps:

[0057] S1: Use waste graphite electrode as raw material A, needle coke as raw material B, homogeneously nucleated mesophase carbon microspheres as raw material C, BFBAEPY-COF self-polymerized ligand as raw material D, and spinning pitch as raw material E; the median particle size D50 of raw material A is 13.62μm; the particle size of raw material B is nanometer-scale, with a particle size range of less than 50nm; the median particle size D50 of raw material C is 7.58μm; the median particle size D50 of raw material D is 20.00μm, and the median particle size D50 of raw material E is 400nm;

[0058] The preparation method of raw material A is to remove the epidermis of the waste graphite electrode, and then sequentially perform crushing, coarse pulverization, fine pulverization, and classification to obtain raw material A; the crushing, coarse pulverization, and fine pulverization are all cutting pulverization;

[0059] S2: According to the mass ratio of raw material D: raw material B: raw material E = 115:13:2.8, raw material D, raw material B and raw material E are mixed by airflow to obtain a mixture F, the mixture F is placed in a reactor, modified at 380°C, the stirring speed of the modification is 75r / min, the modification time is 3h, and cooled to obtain a coated modified material G, and the coated modified material G is heat treated at 750°C for 3h to obtain a coated carbonized material H;

[0060] S3: Raw materials A, C and E are mixed in a mass ratio of 115:38:11 to obtain a mixture I, and the mixture I is dry-milled for 40 min to obtain a ball-milled material J; the ball-milled material J is briquette-formed to obtain a block material K, each block being a cube with a side length of 20 cm; each block of the block material K is wrapped with a graphite paper of 0.8 mm thickness, and then heat-treated at 1350°C for 4 h. After cooling, the graphite paper is removed, and the granulated material L with a median particle size D50 of 20.00 μm is obtained;

[0061] S4: According to the mass ratio of granulated material L: coated carbonized material H: raw material C = 115:32:9, the granulated material L, coated carbonized material H and raw material C are evenly mixed by double cone spiral mixing, passed through a 325 mesh sieve, and the sieve under is taken to obtain a graphite negative electrode material.

[0062] The BFBAEPY-COF self-polymerized ligand used in the above embodiments is produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd. BFBAEPY-COF self-polymerized ligand is a covalent organic framework material (COFs), a crystalline porous polymer, which is a rigid organic structural unit connected by C, H, O, N, and B through covalent bonds to obtain a polymer with regular and ordered pores, which has a conductive effect.

[0063] Comparative Example 1: No coated carbonized material H is prepared, and the coated carbonized material H is replaced by raw material D, and raw material D is mixed with granulated material L and raw material C to obtain a graphite negative electrode material. Other parameters and methods are the same as in Example 1.

[0064] Comparative Example 2: Without preparing granulated material L, raw materials A, C and E are directly heat treated after mixing, cooled, and broken up to obtain powder material, which is mixed with coated carbonized material H and raw material C to obtain graphite negative electrode material. Other parameters and methods are the same as in Example 1.

[0065] Comparative Example 3: Without adding the coated carbonized material H, the granulated material L was mixed with the raw material C to obtain a graphite negative electrode material. Other parameters and methods were the same as in Example 1.

[0066] The performance of the graphite negative electrode materials of the above-mentioned embodiments and comparative examples was tested.

[0067] Prepare LIR2430 button cells, the positive electrode is a lithium sheet, the negative electrode is each graphite negative electrode material, and the compaction density of the negative electrode sheet is 1.68g / m 3 ; Three parallel samples were prepared for each battery; 5C rate charge and discharge test was performed at an ambient temperature of 20°C. The results are shown in Table 1 below:

[0068] Table 1 Graphite anode material performance test results (average value)

[0069]

[0070] It can be seen from the above results that the negative electrode materials of Examples 1 to 5 have good capacity, efficiency and cyclability under the condition of 5C high rate charge and discharge. The graphite negative electrode material of Comparative Example 1 absorbs a large amount of water during slurry mixing, and after the electrode is coated with slurry, dried and compacted, peeling and powdering occur, and the battery cannot be made, and no testing is performed. It can be seen from the results of Comparative Example 2 that the granulated material L has higher capacity and efficiency than the non-granulated material, and can maintain good cyclability. It can be seen from the results of Comparative Example 3 that the addition of coated carbonized material H can improve the capacity and efficiency of the material.

Claims

1. A method for preparing a high-rate graphite negative electrode material, characterized in that: The preparation method comprises the following steps: S1: waste graphite electrode as raw material A, needle coke as raw material B, homogeneous nucleated mesocarbon microspheres as raw material C, BFBAEPY-COF self-polymerized ligand as raw material D, spinning pitch as raw material E; The median particle size D50 of the raw material A is 10 μm to 16 μm; the particle size of the raw material B is nanometer-level, less than 50 nm; the median particle size D50 of the raw material C is 5 μm to 10 μm; the median particle size D50 of the raw material D is 12 μm to 20 μm, and the median particle size D50 of the raw material E is less than 1 μm; S2: According to the mass ratio of raw material D: raw material B: raw material E = (100-120): (6-15): (1.5-3), raw material D, raw material B and raw material E are mixed by airflow to obtain a mixed material F, the mixed material F is placed in a reactor, modified at 300°C-400°C, cooled to obtain a coated modified material G, and the coated modified material G is heat-treated at 650°C-800°C to obtain a coated carbonized material H; S3: Raw materials A, C and E are mixed according to the mass ratio of raw material A: raw material C: raw material E = (100-120): (30-40): (8-12) to obtain a mixture I, and the mixture I is dry-milled for 30-40 minutes to obtain a ball-milled material J; the ball-milled material J is briquette-formed to obtain a block material K, each block being a cube with a side length of 10 cm to 20 cm; each block of the block material K is wrapped with graphite paper, and then heat-treated at 1200°C to 1400°C. After cooling, the graphite paper is removed, and the granulated material L is obtained after crushing and classification; S4: According to the mass ratio, granulated material L: coated carbonized material H: raw material C = (100-120): (25-35): (6-10), the granulated material L, coated carbonized material H and raw material C are mixed evenly, passed through a 300-325 mesh sieve, and the sieve under is taken to obtain a graphite negative electrode material.

2. The method for preparing a high-rate graphite negative electrode material according to claim 1, characterized in that: In S1, the preparation method of the raw material A is to remove the epidermis of the discarded graphite electrode, and then sequentially perform crushing, coarse grinding, fine grinding and classification to obtain the raw material A; the crushing, coarse grinding and fine grinding are all cutting grinding.

3. The method for preparing a high-rate graphite negative electrode material according to claim 1, characterized in that: In S2, the modified stirring speed is 60 r / min to 80 r / min.

4. The method for preparing a high-rate graphite negative electrode material according to claim 1, characterized in that: In S2, the modification time is 2h to 3h.

5. The method for preparing a high-rate graphite negative electrode material according to claim 1, characterized in that: In S2, the heat treatment time is 2h to 3h.

6. The method for preparing a high-rate graphite negative electrode material according to claim 1, characterized in that: In S3, the thickness of the graphite paper is 0.5 mm to 1 mm.

7. The method for preparing a high-rate graphite negative electrode material according to claim 1, characterized in that: In S3, the heat treatment time is 3h to 4h.

8. The method for preparing a high-rate graphite negative electrode material according to claim 1, characterized in that: In S3, the median particle size D50 of the pulverization and classification is 16 μm to 20 μm.

9. The method for preparing a high-rate graphite negative electrode material according to claim 1, characterized in that: In S4, the mixing is carried out by double cone helix mixing.