A rotating tube prepared by using modified expanded graphite and its application

By modifying the expanded graphite slurry, the porous sponge is treated with borax and barium nitrate to form a stable network structure, the pore problem after the carrier is burned is solved, and the thermal shock resistance of the rotating tube is improved, so that it can heat it multiple times Stabilize during the earthquake cycle.

CN118619659BActive Publication Date: 2024-11-29HUNAN KIBING PHARMACEUTICAL MATERIAL TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410847122.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-29
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

In the prior art, porous sponge body has millimeter-level pores after the carrier is burned out, resulting in stress concentration and crack expansion, and poor thermal shock resistance.

Method used

The porous sponge is treated with modified expanded graphite slurry, and a stable [BO4] network structure is formed by reacting borax and barium nitrate with expanded graphite, supporting the pore structure and bridging large pores during the sintering process to form a high-stability Rotate the tube.

Benefits of technology

The thermal shock resistance of the rotating tube is significantly improved, and it can resist multiple thermal shock cycles, and the pore structure stability and large pore bridging are improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of glass production equipment, and in particular to a rotating tube prepared by using modified expanded graphite and its application, so as to solve the problem of millimeter-level pores existing in the original position of the bearing member after limiting the porous sponge body in the prior art, resulting in poor thermal shock performance. The modified expanded graphite is formed by dissolving borax, barium nitrate and expanded graphite in deionized water, stirring and filtering, and then sintering in a helium atmosphere, and grinding into powder after sintering. The addition of modified expanded graphite can not only ensure the pore stability inside the rotating tube system, but also effectively bridge the large pores formed after the bearing member is burned out.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass production equipment, in particular to a rotary tube prepared by using modified expanded graphite and application thereof. Background Art

[0002] A rotating tube is required in the glass drawing process. A Chinese patent with application number CN202310569554.2 discloses a 3D printed porous medium burn-out hole-forming rotating tube preparation process and mold. The rotating tube is prepared by the porous medium burn-out hole-forming method, and a special mold is used to cooperate with the firing of the rotating tube, which improves the thermal shock resistance and significantly reduces the weight.

[0003] However, the above method uses a support to limit the porous sponge body, thereby effectively controlling the position of the porous sponge body. However, after the support is burned out, millimeter-level pores exist in the original position of the support, which are prone to stress concentration, leading to crack expansion and poor thermal shock resistance. Summary of the invention

[0004] The present invention provides a rotating tube prepared by using modified expanded graphite and application thereof, so as to solve the technical problem existing in the prior art that after limiting the porous sponge body, millimeter-level pores exist in situ on the bearing part, resulting in poor thermal shock performance.

[0005] In order to alleviate the above technical problems, the technical solution provided by the present invention is:

[0006] A rotating tube prepared by using modified expanded graphite, wherein the rotating tube slurry is made of the following raw materials in parts by weight:

[0007] 50-70 parts of high-purity sintered mullite;

[0008] 8-20 parts of talc;

[0009] 7-15 parts of aluminum oxide powder;

[0010] 4-10 parts of silica powder;

[0011] 3-25 parts of binding clay;

[0012] 5-10wt% of modified expanded graphite slurry;

[0013] It is prepared by the following method:

[0014] 1) preparing modified expanded graphite slurry: dissolving borax, barium nitrate and expanded graphite in deionized water, stirring and filtering, and then sintering in a helium atmosphere, grinding into powder after sintering, and then dissolving the modified expanded graphite in water to form modified expanded graphite slurry;

[0015] 2) soaking the porous sponge in modified expanded graphite slurry, and then drying the porous sponge containing the modified expanded graphite slurry in the shade;

[0016] 3) placing the air-dried porous sponge containing the modified expanded graphite slurry into a mold, injecting the rotating tube slurry, and demoulding after air-drying to form a semi-finished product;

[0017] 4) Sintering for the first time until the porous sponge decomposes to leave a porous skeleton composed of modified expanded graphite;

[0018] 5) After the first sintering, a second sintering is performed to heal the large gaps in the rotating tube.

[0019] Furthermore,

[0020] The mass ratio of borax, barium nitrate and expanded graphite is (1-3):(4-6):(20-40).

[0021] Furthermore,

[0022] The mass ratio of borax, barium nitrate and expanded graphite is 2:5:30.

[0023] Furthermore, in the process of preparing the modified expanded graphite slurry, the filtered product is dried and then sintered in a high-pressure helium atmosphere.

[0024] Furthermore,

[0025] The first sintering temperature is 1200-1500 degrees Celsius.

[0026] Furthermore,

[0027] The second sintering temperature is 800-1000 degrees Celsius.

[0028] The effect analysis is as follows:

[0029] Expanded graphite is a carbonaceous raw material made by chemical or electrochemical intercalation of natural flake graphite, and then instantaneously heated to produce high-temperature expansion. Expanded graphite has a well-developed pore structure, but it is prone to collapse and agglomeration.

[0030] First, the modified expanded graphite is prepared by using borax and barium nitrate. First, borax provides B atoms. B2O3 is a network former. Since it has two coordination forms, [BO3] and [BO4], when there is sufficient free oxygen in the network, B2O3 will form [BO4] units; when there is insufficient free oxygen, [BO3] units will be formed. Barium nitrate (Ba(NO3)2) will decompose into barium oxide (BaO), nitrogen dioxide (NO2) and oxygen (O2) when heated, which can provide a large amount of free oxygen. The presence of free oxygen will accelerate the transformation of [BO3] units to [BO4] units. [BO4] is a stable network structure like [SiO4]. A large amount of [BO4] network structure in the pores of expanded graphite can effectively support the expanded graphite and prevent the expanded graphite from collapsing and agglomerating, that is, it can better ensure the pore stability inside the rotating tube system. The stable pore structure is conducive to the improvement of thermal shock resistance.

[0031] Secondly, the [BO3] unit body transforms into the [BO4] unit body, and this transformation process is accompanied by volume expansion, so it can effectively bridge the large pores formed after the carrier is burned out.

[0032] In other words, the addition of modified expanded graphite can not only ensure the pore stability inside the rotating tube system but also effectively bridge the large pores formed after the burning of the supporting parts. DETAILED DESCRIPTION

[0033] Example 1

[0034] This embodiment provides a rotating tube prepared by using modified expanded graphite, which is prepared by the following method:

[0035] 1) preparing a modified expanded graphite slurry: dissolving borax, barium nitrate and expanded graphite in deionized water in a weight ratio of 2:5:30, stirring and filtering, and then sintering in a helium atmosphere, grinding into powder after sintering, and then dissolving the modified expanded graphite in water to form a modified expanded graphite slurry;

[0036] 2) soaking the porous sponge in modified expanded graphite slurry, and then drying the porous sponge containing the modified expanded graphite slurry in the shade;

[0037] 3) placing the air-dried porous sponge containing the modified expanded graphite slurry into a mold, injecting the rotating tube slurry, and demoulding after air-drying to form a semi-finished product;

[0038] 4) Sintering for the first time until the porous sponge decomposes to leave a porous skeleton composed of modified expanded graphite;

[0039] 5) After the first sintering, a second sintering is performed to heal the large gaps in the rotating tube.

[0040] in,

[0041] The rotary tube slurry is made from the following raw materials in parts by weight:

[0042] 50-70 parts of high-purity sintered mullite;

[0043] 8-20 parts of talc;

[0044] 7-15 parts of aluminum oxide powder;

[0045] 4-10 parts of silica powder;

[0046] 3-25 parts of binding clay;

[0047] 5-10wt% of modified expanded graphite slurry;

[0048] The shape of the porous sponge in this embodiment adopts the structure in the applicant's previous patent (CN202310569554.2).

[0049] By observing the cross section of the sample, it was found that the pores were evenly distributed at the position corresponding to the porous sponge.

[0050] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process could withstand 36 thermal shock cycles.

[0051] Comparative Example 1

[0052] The modified expanded graphite ratio in this embodiment is different from that in Example 1, specifically:

[0053] Borax: barium nitrate: expanded graphite = 7:0:30, and the rest are the same.

[0054] Observation of the sample cross section revealed that a large number of large pores (greater than 1 mm) appeared at the location corresponding to the porous sponge. The possible reason is that without the presence of barium nitrate, there is insufficient free oxygen in the system and insufficient [BO4] network structure, so the system's support capacity for expanded graphite is insufficient, and the expanded graphite collapses and agglomerates.

[0055] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process can withstand 25 thermal shock cycles. The expanded graphite system is unstable and has large pores, which is not conducive to the stable transfer of thermal energy.

[0056] Comparative Example 2

[0057] The modified expanded graphite ratio in this embodiment is different from that in Example 1, specifically:

[0058] Borax: barium nitrate: expanded graphite = 0:7:30, and the rest are the same.

[0059] Observation of the sample cross section revealed that a large number of large pores (greater than 1 mm) appeared at the location corresponding to the porous sponge. The possible reason is that without the presence of borax, there are no [BO3] units and [BO4] units in the system, so the system's support capacity for expanded graphite is insufficient, and the expanded graphite collapses and agglomerates.

[0060] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process can withstand 24 thermal shock cycles. The expanded graphite system is unstable and has large pores, which is not conducive to the transfer of thermal energy stability.

[0061] Comparative Example 3

[0062] The expanded graphite in this embodiment is not modified, and the rest is the same.

[0063] By observing the cross section of the sample, it was found that a large number of large pores (larger than 1 mm) appeared at the position corresponding to the porous sponge.

[0064] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process can withstand 26 thermal shock cycles. The expanded graphite system is unstable and has large pores, which is not conducive to the stable transfer of thermal energy.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A rotating tube prepared by using modified expanded graphite, characterized in that: The rotary tube slurry is made from the following raw materials in parts by weight: 50-70 parts of high-purity sintered mullite; 8-20 parts of talc; 7-15 parts of aluminum oxide powder; 4-10 parts of silica powder; 3-25 parts of binding clay; 5-10 parts of modified expanded graphite slurry; It is prepared by the following method: 1) Prepare modified expanded graphite slurry: dissolve borax, barium nitrate and expanded graphite in deionized water, stir and filter, then sinter in a helium atmosphere, grind into powder after sintering, and then dissolve the modified expanded graphite in water to form modified expanded graphite slurry; the mass ratio of borax, barium nitrate and expanded graphite is (1-3): (4-6): (20-40); 2) soaking the porous sponge in a modified expanded graphite slurry, and then drying the porous sponge containing the modified expanded graphite slurry in the shade; 3) Place the air-dried porous sponge containing modified expanded graphite slurry into the mold, inject the rotating tube slurry, air-dry to form a semi-finished product, and then demould; 4) The first sintering is performed until the porous sponge decomposes, leaving a porous skeleton composed of modified expanded graphite; 5) After the first sintering, a second sintering is performed to heal the large gaps in the rotating tube. The second sintering temperature is 800-1000 degrees Celsius.

2. The rotating tube prepared by using modified expanded graphite according to claim 1, characterized in that: The mass ratio of borax, barium nitrate and expanded graphite is 2:5:

30.

3. The rotating tube prepared by using modified expanded graphite according to claim 2, characterized in that: In the process of preparing the modified expanded graphite slurry, the product is filtered, dried and then sintered in a high-pressure helium atmosphere.

4. The rotating tube prepared by using modified expanded graphite according to claim 3, characterized in that: The first sintering temperature is 1200-1500 degrees Celsius.

5. Use of a rotating tube prepared by using modified expanded graphite as claimed in any one of claims 1 to 4 in glass production.

Citation Information

Patent Citations

  • 3D printing porous medium burn-out hole-forming rotating tube preparation process and mold

    CN117024172B

  • 3D printing porous medium ignition loss pore-forming rotary tube preparation process and mold

    CN117024172A