Negative electrode current collector and preparation method thereof and battery

By using porous material particles and metal conductive layers in the negative electrode structure to form a three-dimensional network structure and covering the ceramic layer, the problems of lithium ion deposition inequality and insufficient structural strength are solved, and the safety performance and energy density of the battery are significantly improved. .

CN118630226BActive Publication Date: 2024-12-03JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411096502.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-12-03
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Uneven deposition of lithium ions in the negative electrode structure leads to the formation of lithium dendrites, causing safety risks, and the improvement of structural strength and energy density of the prior art is limited.

Method used

The base layer and the ceramic layer coated on the thickness direction of the substrate layer are used to form a three-dimensional network structure and a ceramic layer coated on both surfaces of the substrate layer thickness. The base layer includes porous material particles, a first metal conductive layer and a second metal carbide to form a three-dimensional network structure and the carbon particles are filled. In the pores, the ceramic layer reinforces the structure.

Benefits of technology

It significantly improves the uniformity and structural strength of lithium ion deposition, reduces the growth of lithium dendrites, and enhances the safety performance and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118630226B_ABST
    Figure CN118630226B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of new energy batteries, and specifically to a negative electrode-free current collector, a preparation method thereof, and a battery. The negative electrode-free current collector of the present invention comprises a substrate layer and a ceramic layer coated on two surfaces of the substrate layer in the thickness direction; wherein the substrate layer comprises: substrate particles, the substrate particles comprising porous material particles and a first metal conductive layer coated on the surface of the porous material particles; a second metal carbide, the second metal carbide and the substrate particles form a three-dimensional network structure; carbon particles; the carbon particles are filled in the pores of the three-dimensional network structure. The negative electrode-free current collector of the present invention has high conductivity and significantly improved power performance, and has high structural strength and good safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new energy batteries, and in particular to a negative electrode-free current collector, a preparation method thereof, and a battery. Background Art

[0002] In order to improve the energy density of lithium batteries, more and more research efforts are being invested in the weight reduction design of battery cells. The negative electrode-free structure does not require negative electrode active materials, thus greatly reducing the mass of the battery and improving the energy density of lithium batteries. However, the negative electrode-free structure currently faces a serious problem. Without the lithium embedding of the negative electrode active material, where should the lithium ions released from the positive electrode go? Although the conventional copper foil negative electrode can deposit lithium, it faces the risk of uneven lithium deposition, forming lithium dendrites, piercing the diaphragm, causing a short circuit between the positive and negative electrodes, and causing safety problems.

[0003] In order to solve the problem of uneven lithium deposition in a negative electrode-free battery structure, patent CN113013417A discloses a negative electrode-free structure, in which an electronic conductive layer and an ion conductive layer are coated on the outer layer of a traditional negative electrode material to form an ion-electronic conductive negative electrode structure. Although this method can accommodate the lithium source detached from the positive electrode, the patent adopts a method of directly immersing copper foil in an ion coating gel, and the coating does not have a large number of pores, thereby hindering the deposition rate of lithium ions on the copper foil surface. The efficiency of lithium deposition is low, and in severe cases, lithium ions are deposited on the coating surface due to untimely deposition (high rate charging), causing lithium dendrites to pierce the diaphragm and cause a short circuit; and the ion conductive layer is difficult to prepare, and the traditional negative electrode metal substrate has a large mass, which affects the energy density of the battery. Patent CN116581361A discloses a negative electrode-free structure, which provides lithium insertion space and avoids direct reaction with the electrolyte by setting a lithium titanate layer and inserting lithium in combination with a solid electrolyte. However, the solid electrolyte currently has problems with low ion transfer rate and interface contact, which affects the power performance of the battery. In addition, the setting of the lithium titanate layer also increases weight, which is not conducive to improving the energy density of negative electrode-free batteries. Patent CN114883572A discloses an organic polymer-based membrane with a hollow interior, a metal conductive layer deposited inside, and a self-supporting negative electrode-free structure using a polymer-based membrane. However, the physical adsorption force of the metal layer structure prepared by this method is not strong, and the structure is prone to collapse, which affects the effect of lithium deposition.

[0004] Therefore, how to effectively suppress the uniformity of lithium deposition and improve the structural strength of the negative electrode-free current collector has become a technical problem that needs to be urgently solved for negative electrode-free structure batteries. Summary of the invention

[0005] In view of this, the present invention provides a negative electrode-free current collector and a preparation method thereof and a battery. The negative electrode-free current collector has high conductivity and significantly improved power performance, and has high structural strength and good safety performance.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] In a first aspect, the present invention provides a negative electrode-free current collector, the negative electrode-free current collector comprising a base layer and a ceramic layer coated on two surfaces of the base layer in a thickness direction;

[0008] Wherein, the base layer comprises:

[0009] Base particles, the base particles comprising porous material particles and a first metal conductive layer coated on the surface of the porous material particles;

[0010] a second metal carbide, wherein the second metal carbide and the matrix particles form a three-dimensional network structure;

[0011] Carbon particles; the carbon particles are filled in the pores of the three-dimensional network structure.

[0012] Preferably, the thickness of the substrate layer is 4-20 μm; the thickness of the ceramic layer is 1-5 μm;

[0013] The mass ratio of the matrix particles to the carbon particles is (90-95):(5-10);

[0014] The mass ratio of the matrix particles to the second metal carbide is (99-99.5): (0.5-1).

[0015] Preferably, the particle size of the porous material particles is 0.5-2 μm;

[0016] Preferably, the thickness of the first metal conductive layer is 0.1-0.2 μm;

[0017] Preferably, the second metal element in the second metal carbide is selected from at least one of Group IVB elements, Group VB elements, and Group VIB elements;

[0018] Preferably, the porous material particles are ZIF material particles;

[0019] Preferably, the ZIF material is selected from at least one of ZIF-8, ZIF-60 and ZIF-90;

[0020] Preferably, the first metal in the first metal conductive layer includes at least one of copper, nickel, silver and tungsten;

[0021] Preferably, the second metal carbide is selected from at least one of titanium carbide, tungsten carbide and zirconium carbide.

[0022] Preferably, the ceramic layer comprises inorganic ceramic and a second binder;

[0023] Preferably, the inorganic ceramic includes at least one of aluminum oxide, chromium oxide and zirconium oxide;

[0024] Preferably, the mass ratio of the inorganic ceramic to the second binder is (90-95):(5-10);

[0025] Preferably, the second binder is selected from at least one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber and polyacrylic acid.

[0026] In a second aspect, the present invention provides a method for preparing the above-mentioned negative electrode-free current collector, the preparation method comprising the following steps:

[0027] S1, using a molten liquid of a first metal to perform a deposition treatment on the surface of porous material particles to obtain matrix particles;

[0028] S2, mixing the base particles, the first binder, and the first solvent to obtain a first slurry, curing the first slurry to obtain a first base film; immersing the first base film in a second metal salt solution to obtain a second base film; and subjecting the second base film to a high-temperature treatment with an alkane gas to obtain a base layer;

[0029] S3, performing a second mixing of the inorganic ceramic, the second binder, and the second solvent to obtain a second slurry, and applying the second slurry to the surfaces of both sides of the base layer.

[0030] In an embodiment of the present invention, the first solvent is selected from at least one of water, N-methylpyrrolidone, and dimethylformamide;

[0031] Preferably, the second solvent is selected from N-methylpyrrolidone and / or dimethylformamide.

[0032] In an embodiment of the present invention, the second metal salt is selected from a halide of a second metal;

[0033] Preferably, the second metal salt is a chloride of the second metal;

[0034] Preferably, the molar concentration of the second metal salt solution is 0.01-0.5 mol / L.

[0035] In an embodiment of the present invention, the first binder is selected from at least one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber, and polyacrylic acid;

[0036] Preferably, the mass ratio of the matrix particles to the first binder is (90-95):(5-10).

[0037] In a specific embodiment of the present invention, in step S1, the deposition process is selected from one of spray drying or hot melt sputtering;

[0038] In step S2, the first mixing pressure is -90 to -45 KPa, and the time is 2 to 4 hours;

[0039] The curing temperature is 40-100°C;

[0040] The immersion treatment temperature is 20-40°C and the time is 0.5-2h;

[0041] The high temperature treatment is carried out in an inert gas atmosphere, the temperature of the high temperature treatment is 800-1400° C., and the time is 2-6 hours.

[0042] In a third aspect, the present invention provides a battery, comprising the above-mentioned negative electrode-free current collector and / or the negative electrode-free current collector prepared according to the above-mentioned preparation method.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] 1. The first metal conductive layer coated on the surface of the porous material particles in the present invention has strong conductivity, so that it can have conductivity and negative charge, attract lithium ions during the charging and discharging process, and promote the movement of lithium ions to its surface; the porous material particles can provide a large number of pores, provide a large amount of space for the deposition of lithium ions, and improve the safety of lithium deposition. Furthermore, the porous material particles can be selected from ZIF material particles, which can have the function of absorbing harmful gases, thereby comprehensively improving the safety performance of lithium batteries.

[0045] 2. The second metal carbide in the present invention forms a three-dimensional network structure with the matrix particles, which can effectively enhance the structural strength of the negative electrode-free current collector and prevent it from breaking and falling off.

[0046] 3. The ceramic layer coated on both surfaces of the substrate layer in the thickness direction of the present invention can further improve the growth of lithium dendrites.

[0047] 4. The negative electrode-free current collector of the present invention comprises a substrate layer and a ceramic layer coated on two surfaces of the substrate layer in the thickness direction, wherein the substrate layer comprises substrate particles, a second metal carbide and carbon particles, and the substrate particles comprise porous material particles and a first metal conductive layer coated on the surface of the porous material particles. Through the synergistic effect of the above structures, the safety performance of the negative electrode-free current collector and the safety performance of the battery are jointly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1It is a structural schematic diagram of a negative electrode-free current collector. Specifically, the negative electrode-free current collector includes a base layer and a ceramic layer coated on two surfaces of the base layer in the thickness direction, wherein the base layer includes base particles and a second metal carbide, and the base particles include porous material particles and a first metal conductive layer coated on the surface of the porous material particles.

[0049] Figure 2 It is a schematic diagram of the structure of the base particle. Specifically, the base particle includes a porous material particle and a first metal conductive layer coated on the surface of the porous material particle.

[0050] Description of Reference Numerals

[0051] 1. Matrix particles

[0052] 2. Second metal carbide

[0053] 3. Ceramic layer

[0054] 4. Porous material particles

[0055] 5. The first metal conductive layer DETAILED DESCRIPTION

[0056] The present invention discloses a negative electrode-free current collector and a preparation method and a battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0057] In the description of the present invention, it should be noted that the terms "first", "second", etc. are only used for descriptive purposes, and do not indicate or imply relative importance.

[0058] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0059] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0060] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0061] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0062] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0063] In order to effectively suppress the uniformity of lithium deposition and improve the structural strength of the non-negative electrode current collector, the present invention coats the ceramic layer on both surfaces in the thickness direction of the substrate layer, and coats the first metal conductive layer on the surface of the porous material particles to form substrate particles to suppress the uniformity of lithium deposition, and the second metal carbide forms a three-dimensional network structure with the substrate particles to improve the structural strength of the non-negative electrode current collector. Specifically, the present invention adopts the following technical solutions:

[0064] In a first aspect, the present invention provides a negative electrode-free current collector, the negative electrode-free current collector comprising a base layer and a ceramic layer coated on two surfaces of the base layer in a thickness direction;

[0065] Wherein, the base layer comprises:

[0066] Base particles, the base particles comprising porous material particles and a first metal conductive layer coated on the surface of the porous material particles;

[0067] a second metal carbide, wherein the second metal carbide and the matrix particles form a three-dimensional network structure;

[0068] Carbon particles; the carbon particles are filled in the pores of the three-dimensional network structure.

[0069] The negative electrode-free current collector provided by the present invention improves the conductivity of the negative electrode-free current collector through porous material particles and the first metal conductive layer coated on the surface of the porous material particles, so that it attracts lithium ions during the charge and discharge process and promotes the movement of lithium ions to its surface; the porous material particles can provide a large number of pores, provide a large amount of space for the deposition of lithium ions, and improve the safety of lithium deposition. At the same time, the second metal carbide and the matrix particles form a three-dimensional network structure, which effectively enhances the structural strength of the negative electrode-free current collector and avoids its breakage and falling off; the ceramic layer coated on the two surfaces in the thickness direction of the matrix layer can further improve the growth of lithium dendrites; the present invention improves the safety performance of the negative electrode-free current collector and the safety performance of the battery through the synergistic effect of the above structures.

[0070] In the present invention, the appropriate thickness of the substrate layer can provide a large amount of space for the deposition of lithium ions while reducing the risk of short circuits; shortening the diffusion path of lithium ions to the center, thereby reducing diffusion impedance and improving the power performance of the battery. Preferably, the thickness of the substrate layer can be 4 to 20 μm; the thickness of the ceramic layer can be 1 to 5 μm. In an embodiment of the present invention, the thickness of the substrate layer can be any value of 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, or any value within the range of any two of the above values; the thickness of the ceramic layer can be any value of 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, or any value within the range of any two of the above values.

[0071] Preferably, the mass ratio of the matrix particles to the carbon particles may be (90-95): (5-10); the mass ratio of the matrix particles to the second metal carbide may be (99-99.5): (0.5-1). Within this preferred range, on the one hand, the adverse effect on the conductivity caused by too low a content of carbon particles can be reduced, thereby improving the power performance of the battery; on the other hand, the adverse effect on the embedding of lithium ions caused by too low a proportion of matrix particles can be reduced, thereby improving the safety performance of the battery.

[0072] In the present invention, the particle size of the appropriate porous material particles can increase the strength of the overall structure of the matrix material and increase the space for accommodating lithium ions; the appropriate thickness of the first metal conductive layer helps to further improve the conductivity of the negative electrode-free current collector. In a preferred embodiment of the present invention, the particle size of the porous material particles can be 0.5~2μm; the thickness of the first metal conductive layer can be 0.1~0.2μm. Exemplarily, the particle size of the porous material particles is any value in 0.5μm, 0.75μm, 1.0μm, 1.25μm, 1.5μm, 1.75μm, 2.0μm or any value in the range of any two of the above values; the thickness of the first metal conductive layer is any value in 0.1μm, 0.12μm, 0.14μm, 0.16μm, 0.18μm, 0.2μm or any value in the range of any two of the above values.

[0073] In an embodiment of the present invention, the second metal element in the second metal carbide can be selected from at least one of Group IVB elements, Group VB elements, and Group VIB elements; preferably, in order to enhance the structural strength of the three-dimensional network structure formed by the second metal carbide and the matrix particles, the second metal carbide is selected from at least one of titanium carbide, tungsten carbide, and zirconium carbide.

[0074] Preferably, the porous material particles are ZIF material particles, which can absorb harmful gases and comprehensively improve the safety performance of lithium batteries. Exemplarily, the ZIF material can be selected from at least one of ZIF-8, ZIF-60, and ZIF-90.

[0075] Exemplarily, the porous material particles used in the present invention can be prepared by the following method: mixing a metal salt and an imidazole compound and dissolving them in a solvent to obtain a mixed solution; heating and stirring the mixed solution to obtain a porous material; and ball milling the porous material to obtain porous material particles. The imidazole compound can be 2-methylimidazole; the solvent can be selected from one of water, DMF, ethylene glycol, and methanol; the concentration range of the mixed solution can be 5-20 g / L; the conditions for the heating and stirring treatment can include: a temperature of 100-200°C and a time of 1-6 hours.

[0076] Preferably, the first metal in the first metal conductive layer may include at least one of copper, nickel, silver and tungsten.

[0077] In an embodiment of the present invention, the ceramic layer may include an inorganic ceramic and a second binder.

[0078] Preferably, the inorganic ceramic may include at least one of aluminum oxide, chromium oxide and zirconium oxide.

[0079] Preferably, the mass ratio of the inorganic ceramic to the second binder is (90-95):(5-10).

[0080] Preferably, the second binder is selected from at least one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber and polyacrylic acid.

[0081] In a second aspect, the present invention provides a method for preparing the above-mentioned negative electrode-free current collector, the preparation method comprising the following steps:

[0082] S1, using a molten liquid of a first metal to perform a deposition treatment on the surface of porous material particles to obtain matrix particles;

[0083] S2, mixing the base particles, the first binder, and the first solvent to obtain a first slurry, curing the first slurry to obtain a first base film; immersing the first base film in a second metal salt solution to obtain a second base film; and subjecting the second base film to a high-temperature treatment with an alkane gas to obtain a base layer;

[0084] S3, performing a second mixing of the inorganic ceramic, the second binder, and the second solvent to obtain a second slurry, and applying the second slurry to the surfaces of both sides of the base layer.

[0085] In an embodiment of the present invention, the first solvent may be selected from at least one of water, N-methylpyrrolidone and dimethylformamide; the second solvent is selected from N-methylpyrrolidone and / or dimethylformamide.

[0086] In an embodiment of the present invention, the second metal salt may be selected from a halide of a second metal; preferably, the second metal salt is a chloride of the second metal.

[0087] In an embodiment of the present invention, the molar concentration of the second metal salt solution may be 0.01 to 0.5 mol / L. Exemplarily, the molar concentration of the second metal salt solution is any value among 0.01 mol / L, 0.05 mol / L, 0.10 mol / L, 0.15 mol / L, 0.20 mol / L, 0.25 mol / L, 0.30 mol / L, 0.35 mol / L, 0.40 mol / L, 0.45 mol / L, 0.5 mol / L, or any value within the range consisting of any two of the above values.

[0088] In an embodiment of the present invention, the first binder may be selected from at least one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber, and polyacrylic acid.

[0089] Preferably, the mass ratio of the matrix particles to the first binder is (90-95):(5-10).

[0090] In a specific embodiment of the present invention, in step S1, the deposition process can be selected from spray drying or hot melt sputtering. The present invention can control the deposition thickness of the metal layer by the number and time of deposition.

[0091] In a specific embodiment of the present invention, in step S2, the pressure of the first mixture can be -90~ -45KPa, and the time is 2~4h; the curing treatment in the present invention specifically includes applying the first slurry to the template and curing it at an appropriate temperature; the temperature of the curing treatment can be 40~100℃; the temperature of the impregnation treatment can be 20~40℃, and the time can be 0.5~2h; the high-temperature treatment is carried out in an inert gas atmosphere, and through the high-temperature treatment, the first metal on the surface of the matrix particles reacts with the second metal carbide to form a three-dimensional network structure, and the temperature of the high-temperature treatment can be 800~1400℃, and the time can be 2~6h.

[0092] In a third aspect, the present invention provides a battery, comprising the above-mentioned negative electrode-free current collector and / or the negative electrode-free current collector prepared according to the above-mentioned preparation method.

[0093] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.

[0094] The present invention has no particular restrictions on the positive electrode sheet, separator, and electrolyte in the battery, and those skilled in the art can select them according to actual needs as long as the purpose of the present application can be achieved.

[0095] The reagents, instruments or materials used in the present invention can be obtained through commercial channels.

[0096] The present invention will be further described below in conjunction with embodiments:

[0097] Example 1

[0098] 1. Preparation of matrix particles: Cobalt salt and 2-methylimidazole are uniformly mixed in a solvent such as water at a mass ratio of 1:4 to form a mixed solution of a certain concentration, the solution concentration range is 10g / L, slowly heated to 140°C, stirred and reacted for 3h, and ZIF material can be obtained; the prepared ZIF material is ball-milled to obtain ZIF material particles of a suitable size of 2μm. After the copper metal is thermally melted, it is uniformly deposited on the surface of the ZIF material particles by spray drying or hot melt sputtering to obtain ZIF material particles coated with a copper conductive layer. The deposition thickness of the metal layer is controlled by the deposition number and time. The final deposition thickness of the copper conductive layer is 0.1μm. After cooling, the matrix particles of this embodiment are obtained.

[0099] 2. Preparation of the substrate layer: First, the prepared substrate particles and binder (polyvinylidene fluoride) are uniformly mixed together in a mass ratio of 95%:5%, and vacuum stirred for 2 hours to mix evenly. The mixed slurry is applied to the template and cured at 80°C. The formed substrate film is then immersed in a titanium tetrachloride solution with a concentration of 0.1 mol / L, stirred and immersed for 1 hour, and then the immersed substrate film is taken out and, under N2 protection conditions, an alkane gas is introduced for high-temperature treatment at a temperature of 800°C and a high-temperature treatment time of 2 hours to obtain the substrate layer of this embodiment.

[0100] 3. Finally, the inorganic ceramic and the second binder are uniformly mixed in a ratio of 90%:10%, wherein the inorganic ceramic is alumina and the second binder is polyvinylidene fluoride, and a layer of inorganic ceramic base film with a thickness of about 2 μm is coated on both surfaces in the thickness direction of the substrate layer to obtain the final negative electrode-free current collector of the present invention. The structural schematic diagrams of the negative electrode-free current collector and the substrate particles are shown as follows: Figure 1 and Figure 2 It should be noted that Figure 1 Only the matrix particles and the second metal carbide and their possible positional relationship are shown. The matrix layer should also include irregular carbon particles formed after the first binder is sintered. The carbon particles fill the gaps in the three-dimensional network structure formed by the matrix particles and the second metal carbide.

[0101] 4. Preparation of positive electrode sheet: The positive electrode active material NCM811 (nickel cobalt manganese oxide), the conductive agent is SP (conductive carbon black) and carbon nanotubes, the adhesive is PVDF5130 (polyvinylidene fluoride), and the positive electrode current collector is 13μm aluminum foil. The positive electrode active material, SP, carbon nanotubes, and adhesive are mixed in a ratio of 97:1.5:0.5:1, and NMP (N-methylpyrrolidone) is added and stirred into a uniform and stable positive electrode slurry. The positive electrode slurry is evenly coated on the positive electrode current collector, and the coating surface density is 195g / m 2 After drying and cold pressing, the positive electrode sheet is obtained, and the compaction density is 3.4 g / cm 3 .

[0102] 5. Production of battery cells: Polypropylene film is used as the base film of the isolation membrane, and the thickness of the isolation membrane is 9+3+3+3μm (9μm base film + 3μm ceramic layer + 3μm PVDF coating + 3μm PVDF coating). Arrange the positive electrode sheet, isolation membrane, negative electrode current collector, and isolation membrane in order, and assemble them in sequence by stacking. LiPF6 is dissolved in a solvent with a volume ratio of 1:1:1 of ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate to prepare an electrolyte with a LiPF6 concentration of 1.2 mol / L. Inject the electrolyte into the dry battery cell, soak for 24 hours, and then form it at 45°C. The formation process: charge at 0.05C to 3.4V, and then charge at 0.2C to 3.75V; the battery cell is completed after aging at room temperature for 24 hours.

[0103] Example 2

[0104] The method in this embodiment is the same as that in Embodiment 1, except that the temperature of the high temperature treatment is 1000° C. and the time of the high temperature treatment is 2 h.

[0105] Example 3

[0106] The method in this embodiment is the same as that in Embodiment 1, except that: an inorganic ceramic base film with a thickness of about 4 μm is coated on each of the two surfaces in the thickness direction of the base layer.

[0107] Comparative Example 1

[0108] The method in this comparative example is the same as that in Example 1, except that ZIF material particles not coated with a copper conductive layer are used as base particles.

[0109] Comparative Example 2

[0110] The method in this comparative example is the same as that in Example 1, except that the base film after immersion is not subjected to high temperature treatment and is directly used as the base layer of this comparative example.

[0111] Comparative Example 3

[0112] The method in this comparative example is the same as that in Example 1, except that the temperature of the high temperature treatment is 600° C. and the time of the high temperature treatment is 2 h.

[0113] Comparative Example 4

[0114] The method in this comparative example is the same as that in Example 1, except that the substrate layer after high temperature treatment is not coated with an alumina ceramic coating and is directly used as the negative electrode-free current collector in this comparative example.

[0115] Test Example 1

[0116] The specific surface area, maximum compaction density without negative electrode current collector, weight and conductivity of the matrix particles prepared in the above examples and comparative examples were tested, and the test results are shown in Table 1. The test method is as follows:

[0117] 1. Specific surface area: The specific surface area of ​​the negative electrode-free current collector of the present invention is measured by the N2 adsorption method, and the specific surface area of ​​the material is characterized by the amount of gas adsorption.

[0118] 2. Maximum compaction density: The negative electrode-free current collector of the present invention is sequentially passed through a roller press under different pressure conditions, and at different compaction densities, the SEM and CP of the cross section are used to determine whether the adsorption layer material is broken, thereby obtaining the maximum compaction density.

[0119] 3. Weight: Cut the negative electrode-free current collector of the present invention into a size of 10*10 cm and weigh it.

[0120] 4. Conductivity: The measurement of conductivity is a powder-level resistivity test. A certain amount of matrix particles is placed in a test container, and the same mass of matrix particles is pressed into a dense block under certain pressure conditions, such as 3 to 10 tons of pressure. The resistivity is tested in this state.

[0121] Table 1

[0122]

[0123] As can be seen from Table 1, the specific surface area test shows that the specific surface area of ​​the negative electrode-free current collector is not significantly reduced after the ZIF material particles are coated with a metal layer in the embodiment. This may be because there are fine pores in the metal layer coating. During the specific surface area test, the gas will enter the ZIF material particles through these pores for adsorption. Therefore, the specific surface area structure of the negative electrode-free current collector is not reduced too much; the inorganic ceramic layer of Example 3 is increased to 4μm, which leads to an increase in the specific surface area; the base particles in Comparative Example 1 are not coated with a copper conductive layer, and the exposed ZIF material particles lead to an increase in the specific surface area. And through the conductivity of the embodiment and the comparative example, it can be seen that compared with Comparative Example 1, coating the metal layer on the surface of the ZIF material particles can significantly improve the conductivity of the base particles, which is conducive to promoting the attraction, migration and deposition of lithium ions by improving the conductivity, reducing the internal resistance of the battery, and improving the power performance.

[0124] Test Example 2

[0125] The performance of the batteries prepared in the above embodiments and comparative examples was tested, and the test results are shown in Table 2. The battery performance test method is as follows:

[0126] 1. Internal resistance: Place the battery at 25°C for 30 minutes, charge at 0.5C constant current to 4.25V, charge at constant voltage to 0.05C, place the battery at rest for 30 minutes, discharge at 1C for 30 minutes, place the battery at rest for 60 minutes, then use a multimeter or voltage resistance meter to contact the positive and negative terminals with the positive and negative ears of the battery. The reading on the display is the battery internal resistance at 50% SOC.

[0127] 2. 1C cycle: place the battery at 25℃ for 30min, charge at 0.5C constant current to 4.25V, charge at 0.05C constant voltage, place at 30min, discharge at 1C to 2.5V, record the discharge capacity of the first cycle as the initial capacity, and the capacity retention rate of 500 cycles = discharge capacity of the 500th cycle / discharge capacity of the first cycle.

[0128] 3. 1C energy density = 1C discharge capacity * 1C discharge average voltage / total weight of the battery. The standard test process is: let the battery stand for 30 minutes in a 25℃ environment, charge to 4.25V at 0.5C constant current, charge to 0.05C at constant voltage, let stand for 30 minutes, discharge to 2.5V at 1C, collect the discharge capacity and discharge voltage data of the test, and then the energy density = discharge capacity * average voltage / battery weight.

[0129] 4. Gas volume test: The gas volume test is carried out using the water displacement method and a volume tester. First, the initial weight m1 of the battery cell is weighed, and then the mass m2 after immersion in water is weighed. According to the buoyancy F=ρgV exerted on the battery cell in water, the buoyancy F=m1-m2 at this time, the water density ρ and mass acceleration g are known, so the volume V=(m1-m2) / ρg.

[0130] 5. Hot box test: Place the battery in a 25℃ environment for 30 minutes, charge it to 4.25V at 0.5C constant current, charge it to 0.05C at constant voltage, place the fully charged battery in a hot box, heat it to 130℃ at a rate of 5℃ per minute and keep it for half an hour, observe it for half an hour, if the battery does not catch fire or smoke, continue to heat it at a rate of 5℃ until the battery fails, the temperature at this time is the failure temperature.

[0131] 6. Rate test: Repeat the charge and discharge test of the battery at 1C, 2C, 3C, etc. until the battery has thermal runaway. The rate at this time is the maximum safe rate of the battery without negative electrode current collector, which indirectly reflects the safety performance of the structure without negative electrode current collector. The specific process is: let the battery stand for 30 minutes in a 25℃ environment, charge to 4.25V at 0.5C constant current, charge to 0.05C at constant voltage, stand for 30 minutes, discharge to 2.5V at 1C, stand for 30 minutes, repeat this charge and discharge process, only change the current in 1C discharge to 2.5V to 2C\3C, etc., until the battery has thermal runaway.

[0132] Table 2

[0133]

[0134] It can be seen from Table 2 that the negative electrode-free current collector of the present invention includes porous material particles coated with a conductive layer, which is beneficial to improving the conductivity of the current collector, and is more conducive to promoting the attraction, migration and deposition of lithium ions, and reducing the internal resistance of the battery, improving the power performance, so the internal resistance of the battery prepared by the negative electrode-free current collector of the present invention is reduced to a certain extent, and the cycle efficiency is significantly improved. Under the same structure (including the ceramic layer), the energy density of the battery is significantly improved. And the battery prepared by the present invention has a significantly reduced volume of released gas, a significantly increased failure temperature in the hot box test, and a significantly increased maximum charging rate in the rate test, so the battery prepared by the present invention has significantly improved safety performance.

[0135] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A negative electrode-free current collector, characterized in that: The negative electrode-free current collector comprises a base layer and a ceramic layer coated on two surfaces of the base layer in a thickness direction; Wherein, the base layer comprises: Base particles, the base particles comprising porous material particles and a first metal conductive layer coated on the surface of the porous material particles; the porous material particles are ZIF material particles; the first metal in the first metal conductive layer comprises at least one of copper, nickel, silver and tungsten; A second metal carbide, wherein the second metal carbide and the matrix particles form a three-dimensional network structure; Carbon particles; the carbon particles are filled in the pores of the three-dimensional network structure.

2. The negative electrode-free current collector according to claim 1, characterized in that: The thickness of the substrate layer is 4-20 μm; the thickness of the ceramic layer is 1-5 μm; The mass ratio of the matrix particles to the carbon particles is (90-95):(5-10); The mass ratio of the matrix particles to the second metal carbide is (99-99.5): (0.5-1).

3. The negative electrode-free current collector according to claim 1, characterized in that: The particle size of the porous material particles is 0.5-2 μm; The thickness of the first metal conductive layer is 0.1-0.2 μm; The second metal element in the second metal carbide is selected from at least one of Group IVB elements, Group VB elements and Group VIB elements.

4. The negative electrode-free current collector according to claim 1, characterized in that: The ceramic layer includes inorganic ceramic and a second binder; The inorganic ceramic includes at least one of aluminum oxide, chromium oxide and zirconium oxide; The mass ratio of the inorganic ceramic to the second binder is (90-95):(5-10); The second binder is selected from at least one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber and polyacrylic acid.

5. A method for preparing a negative electrode-free current collector according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: S1, using a molten liquid of a first metal to perform a deposition treatment on the surface of porous material particles to obtain matrix particles; S2, mixing the base particles, the first binder, and the first solvent to obtain a first slurry, curing the first slurry to obtain a first base film; immersing the first base film in a second metal salt solution to obtain a second base film; and subjecting the second base film to a high-temperature treatment with an alkane gas to obtain a base layer; S3, performing a second mixing of the inorganic ceramic, the second binder, and the second solvent to obtain a second slurry, and applying the second slurry to the surfaces of both sides of the base layer.

6. The preparation method according to claim 5, characterized in that: The first solvent is selected from at least one of water, N-methylpyrrolidone, and dimethylformamide; The second solvent is selected from N-methylpyrrolidone and / or dimethylformamide.

7. The preparation method according to claim 5, characterized in that: The second metal salt is selected from a halide of a second metal; The molar concentration of the second metal salt solution is 0.01-0.5 mol / L.

8. The preparation method according to claim 5, characterized in that: The first binder is selected from at least one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber and polyacrylic acid; The mass ratio of the matrix particles to the first binder is (90-95):(5-10).

9. The preparation method according to claim 7, characterized in that: In step S1, the deposition process is selected from one of spray drying or hot melt sputtering; In step S2, the first mixing pressure is -90 to -45 KPa, and the time is 2 to 4 hours; The curing temperature is 40-100°C; The immersion treatment temperature is 20-40°C and the time is 0.5-2h; The high temperature treatment is carried out in an inert gas atmosphere, the temperature of the high temperature treatment is 800-1400° C., and the time is 2-6 hours.

10. A battery, characterized in that: The battery comprises the negative electrode-free current collector according to any one of claims 1 to 4, and / or the negative electrode-free current collector prepared by the preparation method according to any one of claims 5 to 9.