A method for strengthening fluorine separation and recovery in phosphate ore by using microbubbles coupled with silicon additives

By using microbubble coupled silicon additives during the phosphoric acid decomposition process of phosphate ore, the conversion of fluorine into volatile fluoride is strengthened, and the problem of low fluorine resource recovery efficiency in the wet phosphoric acid process is solved, achieving efficient fluorine separation and recovery , reduces the fluorine content in phosphogypsum.

CN118637570BActive Publication Date: 2024-11-12INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114166.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

It is difficult to effectively recover fluorine resources from the phosphate acid decomposition process in the existing wet phosphoric acid process, resulting in excessive fluorine content in phosphogypsum and the existing technology cannot solve the fluorine impurity problem from the source.

Method used

The method of microbubble coupled silicon additives is adopted to strengthen the conversion of fluorine into volatile fluoride during the phosphoric acid decomposition of phosphate ore. Through the synergistic effect of microbubble treatment and the active silicon additives, efficient separation and recovery of fluorine is achieved.

Benefits of technology

Efficient separation and recovery of fluorine was achieved, with the fluorine recovery rate reaching more than 43.9%. Fluorine impurities were separated from the source of phosphate acid decomposition to prevent fluorine from entering the subsequent wet phosphoric acid process, and the fluorine entrainment in phosphogypsum was reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637570B_ABST
    Figure CN118637570B_ABST
Patent Text Reader

Abstract

The present invention provides a method for strengthening the separation and recovery of fluorine in phosphate ore by using microbubbles coupled with silicon additives, the method comprising: mixing phosphate ore, phosphoric acid and active silicon additives to obtain slurry, and subjecting the slurry to microbubble generation treatment to obtain microbubble slurry, the microbubble slurry is circulated back to the reaction, the escaped volatile fluoride is recovered, and defluorination slurry is obtained after the reaction is completed; the obtained defluorination slurry is subjected to acid hydrolysis reaction and solid-liquid separation to obtain phosphoric acid and phosphogypsum. The method provided by the present invention utilizes the synergistic effect of microbubbles and active silicon additives in the phosphoric acid hydrolysis of phosphate ore to strengthen the conversion of fluorine impurities in phosphate ore into volatile fluoride SiF 4 The fluorine impurities can be separated from the acid hydrolysis source of phosphate rock to avoid fluorine from entering the subsequent wet phosphoric acid process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wet-process phosphoric acid and relates to a method for recovering fluorine from phosphate ore, and in particular to a method for strengthening the recovery of fluorine from phosphate ore by using microbubbles coupled with silicon additives. Background Art

[0002] The wet phosphoric acid process is a process for producing phosphoric acid by decomposing phosphate rock with inorganic acid. The main processes of the wet phosphoric acid production process include: acid hydrolysis of phosphate rock with acid (including sulfuric acid, nitric acid, hydrochloric acid, etc.), filtering the reaction slurry after acid hydrolysis to obtain gypsum filter cake and phosphoric acid with low concentration, and the phosphoric acid with low concentration is concentrated to obtain phosphoric acid product. The reaction of the acid hydrolysis process of phosphate rock is actually carried out in two steps. The first step is the pre-decomposition treatment of phosphate rock. The phosphate rock is first dissolved in phosphoric acid to form monocalcium phosphate. The second step is the reaction of the monocalcium phosphate slurry obtained in the previous step with excess sulfuric acid to form a phosphoric acid solution of calcium sulfate crystals.

[0003] With the development of phosphate resources, the resource utilization of medium and low-grade phosphate ores has become an urgent need of the phosphorus chemical industry. In the process of wet phosphoric acid using collophanite, collophanite reacts with acid to hydrolyze, continuously releasing a large amount of impurities such as aluminum, iron, magnesium, sodium, potassium, etc., which are very easy to combine with fluorine to form fluorosilicates or fluoroaluminates. As the reaction continues, fluorosilicates and fluoroaluminates reach an oversaturated state and are easy to precipitate and crystallize, which not only causes a waste of fluorine resources, but also leads to an excessively high fluorine content in phosphogypsum. Therefore, it is of great significance to carry out defluorination recovery in the acid hydrolysis process of phosphate ore.

[0004] CN115285954A discloses a method for improving the fluorine yield in the concentration section of wet-process phosphoric acid production, wherein a defluorinating agent emulsion is added to the dilute phosphoric acid prepared by the wet-process phosphoric acid process, and then fluorosilicic acid is recovered after concentration; CN105236372A discloses a method and device for removing fluorine from wet-process phosphoric acid by air blowing, wherein diatomaceous earth is added to the fluorine-containing wet-process phosphoric acid, and hot air is introduced into the resulting mixed solution, and the fluorine-containing wet-process phosphoric acid is released from the phosphoric acid in the form of gas under the action of hot air and diatomaceous earth. The defluorination process of the prior art usually performs defluorination treatment on the prepared wet-process phosphoric acid, which cannot solve the fluorine impurity problem in the wet-process phosphoric acid process from the source, and the phosphogypsum product will also be mixed with fluorine, resulting in a high fluorine content.

[0005] CN115611248A discloses a method for enhancing the decomposition of phosphate rock with microbubbles, which uses a sulfuric acid acid solution to generate microbubbles to enhance the decomposition of phosphate rock particles and the escape of fluorine-containing gases. However, this method can only enhance the escape of existing fluorine-containing gases, and it is difficult to achieve further conversion of other fluorine-containing substances, and it is difficult to further improve the removal and recovery effect of fluorine.

[0006] Therefore, based on the shortcomings of the existing technology, it is necessary to provide a method for enhancing fluorine conversion and recovery in the acid hydrolysis process of phosphate rock. Summary of the invention

[0007] The object of the present invention is to provide a method for strengthening the separation and recovery of fluorine in phosphate ore by using microbubbles coupled with silicon additives, so as to strengthen the conversion of fluorine into volatile fluoride for separation and recovery during the phosphoric acid hydrolysis of phosphate ore.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for strengthening the separation and recovery of fluorine in phosphate ore by using microbubbles coupled with silicon additives, the method comprising the following steps:

[0010] (1) mixing phosphate rock, phosphoric acid and active silicon additive to react to obtain slurry, and subjecting the slurry to microbubble generation treatment to obtain microbubble slurry, wherein the microbubble slurry is circulated back to the reaction to recover the escaped volatile fluoride, and after the reaction is completed, a defluorinated slurry is obtained;

[0011] (2) The defluorinated slurry obtained in step (1) is subjected to acid hydrolysis and solid-liquid separation to obtain phosphoric acid and phosphogypsum.

[0012] The acid hydrolysis of phosphate rock to produce phosphoric acid and produce phosphogypsum as a by-product is mainly divided into two processes: one is the reaction process between phosphate rock and phosphoric acid (also called premixing or pretreatment), and the other is the acid hydrolysis process between phosphoric acid reaction slurry and sulfuric acid. In the phosphoric acid reaction process, phosphate rock reacts with phosphoric acid to produce calcium dihydrogen phosphate and releases hydrofluoric acid. The reaction equation is as follows:

[0013]

[0014] Since phosphoric acid is weak in acidity, impurity minerals in phosphate rock (quartz, calcium feldspar, potassium feldspar, sodium feldspar, pyrite, etc.) are difficult to react with phosphoric acid, so the release of impurities such as silicon, aluminum, sodium, potassium, and iron is small, and fluorine mainly exists in the form of hydrofluoric acid. During the sulfuric acid acidolysis reaction, sulfuric acid and calcium dihydrogen phosphate in the phosphoric acid reaction slurry continue to react to generate phosphoric acid and phosphogypsum. The reaction mode is as follows:

[0015]

[0016] Due to the strong acidity of sulfuric acid, the impurity minerals that are not decomposed during the phosphoric acid hydrolysis continue to react with sulfuric acid, releasing a large amount of impurities such as silicon, aluminum, iron, magnesium, sodium, potassium, etc., which are very easy to combine with fluorine to form fluorosilicates or fluoroaluminates, etc. The reaction process is as follows:

[0017]

[0018] As the reaction proceeds, fluorosilicates and fluoroaluminates reach an oversaturated state and are prone to precipitate and crystallize, entering the phosphogypsum during the vacuum filtration process. The fluorine in the phosphoric acid obtained by filtration mainly exists in the form of fluorosilicates, fluoroaluminates and a small amount of hydrofluoric acid, which not only causes a waste of fluorine resources, but also leads to an excessively high residual fluorine content in the phosphogypsum.

[0019] In the phosphoric acid reaction process, the silicon-containing impurity minerals (calcium feldspar, potassium feldspar, sodium feldspar, quartz) in the phosphate ore have weak reaction activity and are difficult to react with hydrofluoric acid. The present invention introduces active silicon additives (i.e., active silicates, including soluble silicates, part of colloidal silicon and oligomeric silicates) into the phosphoric acid reaction process, which can directly strengthen the reaction between hydrofluoric acid in the acid solution and the active silicon additives (generally in the form of SiO 2 Expressed in the form of) rapid reaction to generate fluorosilicic acid, the reaction equation is as follows:

[0020]

[0021] The strong shear force generated during the generation of microbubbles and the instantaneous release of pressure when the microbubbles burst will form ultra-high-speed microjets and local ultra-high temperatures and ultra-high pressures. On the one hand, they can strengthen the crushing of active silicon additive particles, promote the reaction dissociation of phosphate rock and the decomposition and release of fluorine, reduce the particle size of active silicon additive particles, increase the reaction area, and accelerate the reaction between hydrofluoric acid and active silicon additives; on the other hand, fluorosilicic acid is very easy to decompose into highly volatile silicon tetrafluoride and hydrogen fluoride under the action of high temperature, strong acidity, local ultra-high temperature / high pressure and microjets generated by the collapse of microbubbles. The reaction equation is as follows:

[0022]

[0023] The gas mass transfer rate inside the microbubbles is extremely fast, which can quickly "bring out" the above-mentioned highly volatile fluorine-containing compounds from the liquid surface (i.e., gas lift effect), thereby achieving fluorine separation.

[0024] Preferably, the composition of the phosphate rock includes: 2 O 5 15-35wt%, F 1.5-4wt%, SiO 2 5-15wt%,Al 2 O 3 1-8wt%Fe 2 O 3 0.1-2wt%, K 2 O 0.1-3wt%,Na 2 O 0.05-1.5wt%.

[0025] In the phosphate rock, P 2 O 5The content is 15-35wt%, for example, it can be 15wt%, 18wt%, 20wt%, 22wt%, 25wt%, 28wt%, 30wt%, 32wt% or 35wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] In the phosphate rock, the F content is 1.5-4.0wt%, for example, it can be 1.5wt%, 2.0wt%, 2.5wt%, 3.0wt%, 3.5wt% or 4.0wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] In the phosphate rock, SiO 2 The content is 5-15wt%, for example, it can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] In the phosphate rock, Al 2 O 3 The content is 1-8wt%, for example, it can be 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt% or 8wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] In the phosphate rock, Fe 2 O 3 The content is 0.1-2wt%, for example, it can be 0.1wt%, 0.3wt%, 0.5wt%, 0.8wt%, 1wt%, 1.2wt%, 1.5wt%, 1.8wt% or 2wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] In the phosphate rock, K 2 The content of O is 0.1-3wt%, for example, 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt% or 3wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] In the phosphate rock, Na 2 The content of O is 0.05-1.5wt%, for example, it can be 0.05wt%, 0.1wt%, 0.3wt%, 0.5wt%, 0.8wt%, 1.0wt%, 1.2wt% or 1.5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the phosphoric acid 2 O 5 The content is 35-55%, for example, it can be 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52% or 55%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the mass ratio of the phosphate rock to phosphoric acid is 1:(1-2), for example, it can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the active silicon additive comprises any one of diatomaceous earth, white carbon black, silicon powder, silica aerogel or nano-silica, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of diatomaceous earth and white carbon black, a combination of white carbon black and silicon powder, a combination of silicon powder and silica aerogel, a combination of silica aerogel and nano-silica, a combination of diatomaceous earth, white carbon black and silicon powder, a combination of silicon powder, silica aerogel and nano-silica, a combination of diatomaceous earth, white carbon black, silicon powder and silica aerogel, or a combination of diatomaceous earth, white carbon black, silicon powder, silica aerogel and nano-silica.

[0035] Preferably, the mass ratio of silicon in the active silicon additive to fluorine in the phosphate rock is (0.5-3):1, for example, it can be 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1 or 3:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the reaction temperature is 95-115°C, for example, it can be 95°C, 98°C, 100°C, 102°C, 105°C, 108°C, 110°C, 112°C or 115°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the reaction time is 1-5 h, for example, 1 h, 2 h, 3 h, 4 h or 5 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the gas-liquid volume ratio of the microbubble generation treatment is 1:(5-10), for example, it can be 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the gas used in the microbubble generation process includes air, N 2 , O 2 or CO 2 Any one or a combination of at least two of the following, a typical but non-limiting combination includes air and N 2 Combination of N 2 With O 2 The combination of O 2 With CO 2 Combination of air, N 2 With O 2 Combination of N 2 , O 2 With CO 2 A combination of, or, air, N 2 , O 2 With CO 2 combination.

[0040] Preferably, the average diameter of the microbubbles is 300-800 μm, for example, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, 550 μm, 600 μm, 650 μm, 700 μm, 750 μm or 800 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] In the present invention, microbubble treatment is carried out by using slurry as a water source and gas as a gas source, which are respectively introduced into a microbubble generating device. The microbubble generating device used can be a conventional microbubble generating device in the art, and the present invention does not limit its specific structure here.

[0042] Preferably, the fluorine content in the volatile fluoride is 1-12 kg / m 3 , for example, it can be 1kg / m 3 , 2kg / m 3 , 4kg / m 3 , 5kg / m 3 , 6kg / m 3 , 8kg / m 3 , 10kg / m 3 or 12kg / m 3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, during the circulation of the microbubble slurry, the mass flow ratio of the microbubble slurry to phosphoric acid is (20-40):1, for example, it can be 20:1, 22:1, 25:1, 28:1, 30:1, 32:1, 35:1, 38:1 or 40:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] Preferably, the acidolysis reaction comprises reacting the defluorination slurry with sulfuric acid.

[0045] Preferably, the temperature of the acid hydrolysis reaction is 80-105°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C or 105°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the mass ratio of sulfuric acid to phosphate rock is (0.6-1.4):1, for example, it can be 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1.0:1, 1.1:1, 1.2:1, 1.3:1 or 1.4:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] Preferably, the acid hydrolysis reaction obtains water to control the P content of the slurry. 2 O 5 The content is 25-40%, for example, it can be 25%, 28%, 30%, 32%, 35%, 38% or 40%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] As a preferred technical solution of the method provided by the present invention, the method comprises the following steps:

[0049] (1) Phosphate rock, phosphoric acid and active silicon additive are mixed and reacted at 95-115℃. 2 O 5 The content of is 15-35wt%, the content of F is 1.5-4wt%, and the content of SiO 2 Content is 5-15wt%, Al 2 O 3 The content of Fe is 1-8wt%, 2 O 3 The content of K is 0.1-2wt%, 2 The content of O is 0.1-3wt%, Na 2 O content is 0.05-1.5wt%, P in phosphoric acid 2 O 5 The content is 35-55%, the mass ratio of phosphate rock to phosphoric acid is 1:(1-2), and the mass ratio of silicon in the active silicon additive to fluorine in the phosphate rock is (0.5-3):1, to obtain a slurry;

[0050] and subjecting the slurry to a microbubble generation process, wherein the gas-liquid volume ratio in the microbubble generation process is 1:(5-10), and the average diameter of the microbubbles is 300-800 μm, to obtain a microbubble slurry;

[0051] The microbubble slurry is circulated back to the reaction, the flow ratio of the microbubble slurry to phosphoric acid is (20-40):1, and volatile fluoride escapes at the same time, and the fluorine content in the volatile fluoride is 1-12kg / m 3 , volatile fluoride is absorbed by spraying with aqueous solution;

[0052] The reaction time is 1-5 hours, and a defluorination slurry is obtained after the reaction is completed;

[0053] (2) The defluorination slurry in step (1) is subjected to an acid hydrolysis reaction with sulfuric acid at 80-105°C, and the mass ratio of sulfuric acid to phosphate rock is (0.6-1.4):1. After the acid hydrolysis reaction, a slurry is obtained, and the P content in the slurry is controlled by adding process water. 2 O 5 The content is 25-40%, and then solid-liquid separation is carried out to obtain phosphoric acid and phosphogypsum, and part of the phosphoric acid is returned to the reaction described in step (1).

[0054] Compared with the prior art, the present invention has the following beneficial effects:

[0055] The method provided by the present invention utilizes the synergistic effect of microbubbles and active silicon additives in the phosphoric acid hydrolysis of phosphate rock to strengthen the conversion of fluorine impurities in the phosphate rock into volatile fluoride SiF 4 The fluorine impurities can be separated from the acid hydrolysis source of phosphate rock to avoid fluorine from entering the subsequent wet phosphoric acid process. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a flow chart of the method provided in Example 1 for enhancing the separation and recovery of fluorine in phosphate ore using microbubbles coupled with silicon additives. DETAILED DESCRIPTION

[0057] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0058] Example 1

[0059] This embodiment provides a Figure 1 The method shown is to use microbubbles coupled with silicon additives to enhance the separation and recovery of fluorine in phosphate ore.

[0060] The composition of phosphate rock includes: 2 O 5 29wt%,F 2.8wt%,SiO 2 10wt%Al 2 O 3 5wt%Fe 2 O3 1wt%,K 2 O0.5wt%,Na 2 O 0.9wt%.

[0061] The method comprises the following steps:

[0062] (1) Phosphate rock, P 2 O 5 Phosphoric acid with a content of 45% and active silicon additive diatomaceous earth are mixed for reaction, wherein the mass ratio of phosphate rock to phosphoric acid is 1:1.8, the mass ratio of diatomaceous earth to phosphate rock according to the mass of silicon to the mass of fluorine is 1.5:1, and the reaction temperature is 110°C;

[0063] (2) The slurry formed in step (1) is used as a water source and air is used as a gas source. The volume ratio of the gas source to the water source is 1:7, and the microbubbles are formed in the slurry. The average diameter of the microbubbles is 500 μm. The slurry containing microbubbles is circulated back to the reaction in step (1). The mass flow ratio of the slurry containing microbubbles to phosphoric acid is 30:1. At the same time, the escaping fluorine content is 8 kg / m 3 The volatile fluoride is then absorbed by spraying with an aqueous solution. The reaction time is 3 hours. After the reaction is completed, a defluorinated slurry is obtained.

[0064] (3) The defluorinated slurry obtained in step (2) is subjected to an acid hydrolysis reaction with sulfuric acid, wherein the mass ratio of sulfuric acid (concentration of 98%) to phosphate rock is 1.1:1, and the P content in the slurry is controlled by adding process water. 2 O 5 The content is 28%, the temperature of the acid hydrolysis reaction is 85°C, and the slurry after the acid hydrolysis reaction is filtered to obtain phosphoric acid and phosphogypsum. According to the amount used, part of the phosphoric acid is returned to the reaction in step (1).

[0065] Example 2

[0066] This embodiment provides a method for enhancing the separation and recovery of fluorine in phosphate ore by using microbubbles coupled with silicon additives.

[0067] The composition of phosphate rock includes: 2 O 5 15wt%,F 1.5wt%,SiO 2 15wt%Al 2 O 3 8wt%Fe 2 O 3 2wt%,K 2 O3wt%,Na 2 O 0.05wt%.

[0068] The method comprises the following steps:

[0069] (1) Phosphate rock, P 2 O 5 Phosphoric acid with a content of 35% and active silicon additives, 50% nano-silicon dioxide and 50% silicon dioxide aerogel are mixed for reaction, wherein the mass ratio of phosphate rock to phosphoric acid is 1:1, the mass ratio of active silicon additive to phosphate rock according to the mass of silicon to the mass of fluorine is 3:1, and the reaction temperature is 115°C;

[0070] (2) The slurry formed in step (1) is used as a water source and nitrogen is used as a gas source. The gas source and the water source are introduced into a microbubble generating device at a volume ratio of 1:5, and microbubbles are formed in the slurry. The average diameter of the microbubbles is 800 μm. The slurry containing microbubbles is circulated back to the reaction in step (1). The mass flow ratio of the slurry containing microbubbles to phosphoric acid is 40:1. At the same time, the escaping fluorine content is 1 kg / m 3 The volatile fluoride is then absorbed by spraying with an aqueous solution. The reaction time is 5 hours. After the reaction is completed, a defluorinated slurry is obtained.

[0071] (3) The defluorinated slurry obtained in step (2) is subjected to an acid hydrolysis reaction with sulfuric acid (concentration of 98%), the mass ratio of sulfuric acid to phosphate rock is 0.6:1, and the P content in the slurry is controlled by adding process water. 2 O 5 The content is 25%, the temperature of the acid hydrolysis reaction is 80°C, and the slurry after the acid hydrolysis reaction is filtered to obtain phosphoric acid and phosphogypsum. According to the amount, part of the phosphoric acid is returned to the reaction in step (1).

[0072] Example 3

[0073] This embodiment provides a method for enhancing the separation and recovery of fluorine in phosphate ore by using microbubbles coupled with silicon additives.

[0074] The composition of phosphate rock includes: 2 O 5 35wt%,F 4wt%,SiO 2 5wt%,Al 2 O 3 1wt%Fe 2 O 3 0.1wt%,K 2 O0.1wt%,Na 2 O 1.5wt%.

[0075] The method comprises the following steps:

[0076] (1) Phosphate rock, P 2 O 5Phosphoric acid with a content of 55% and active silicon additives, 70% white carbon black and 30% silicon powder are mixed for reaction, wherein the mass ratio of phosphate rock to phosphoric acid is 1:2, the mass ratio of active silicon additive to phosphate rock according to the mass of silicon to the mass of fluorine is 0.5:1, and the reaction temperature is 95°C;

[0077] (2) The slurry formed in step (1) is used as a water source, and 50% O 2 and 50% CO 2 The gas source is used as the gas source, and the volume ratio of the gas source to the water source is 1:10, respectively entering the microbubble generating device, forming microbubbles in the slurry, and the average diameter of the microbubbles is 300 μm. The slurry containing microbubbles is circulated back to the reaction in step (1), and the mass flow ratio of the slurry containing microbubbles to phosphoric acid is 20:1. At the same time, the escaping fluorine content is 12 kg / m 3 The volatile fluoride is then absorbed by spraying with an aqueous solution. The reaction time is 1 hour. After the reaction is completed, a defluorinated slurry is obtained.

[0078] (3) The defluorinated slurry obtained in step (2) is subjected to an acid hydrolysis reaction with sulfuric acid (concentration of 98%), the mass ratio of sulfuric acid to phosphate rock is 1.4:1, and the P content in the slurry is controlled by adding process water. 2 O 5 The content is 40%, the temperature of the acid hydrolysis reaction is 105°C, and the slurry after the acid hydrolysis reaction is filtered to obtain phosphoric acid and phosphogypsum. According to the amount used, part of the phosphoric acid is returned to the reaction in step (1).

[0079] Example 4

[0080] This embodiment provides a method for enhancing the separation and recovery of fluorine in phosphate ore by using microbubbles coupled with silicon additives. Compared with Example 1, the temperature of the reaction in step (1) is controlled to be 85° C., and the rest is the same as Example 1.

[0081] Example 5

[0082] This embodiment provides a method for enhancing the separation and recovery of fluorine in phosphate ore by using microbubbles coupled with silicon additives. Compared with Embodiment 1, the temperature of the reaction in step (1) is controlled to be 125° C., and the rest is the same as Embodiment 1.

[0083] Example 6

[0084] This embodiment provides a method for strengthening the separation and recovery of fluorine in phosphate rock by using microbubbles coupled with silicon additives. Compared with Example 1, the P of phosphoric acid in step (1) is controlled. 2 O 5 The content is 25%, and the rest is the same as in Example 1.

[0085] Example 7

[0086] This embodiment provides a method for strengthening the separation and recovery of fluorine in phosphate rock by using microbubbles coupled with silicon additives. Compared with Example 1, the P of phosphoric acid in step (1) is controlled. 2 O 5 The content is 65%, and the rest is the same as in Example 1.

[0087] Comparative Example 1

[0088] This comparative example provides a method for enhancing the separation and recovery of fluorine in phosphate ore by using microbubbles.

[0089] The phosphate rock used is the same as that in Example 1.

[0090] The method comprises the following steps:

[0091] (1) Phosphate rock, P 2 O 5 Phosphoric acid with a content of 45% is mixed for reaction, wherein the mass ratio of phosphate rock to phosphoric acid is 1:1.8, the reaction temperature is 110°C, the reaction time is 3h, and a slurry is obtained after the reaction is completed;

[0092] (2) The slurry obtained in step (1) is mixed with sulfuric acid for acid hydrolysis reaction, the mass ratio of sulfuric acid to phosphate rock is 1.1:1, and the P content in the slurry is controlled by adding process water. 2 O 5 The content is 28%, the temperature of the acidolysis reaction is 85°C, the slurry obtained after the acidolysis reaction is used as the water source, and the air is used as the gas source. The gas source and the water source enter the microbubble generating device according to the volume ratio of 1:7, and microbubbles are formed in the slurry. The average diameter of the microbubbles is 500μm. The slurry containing microbubbles is circulated back to the acidolysis reaction. The mass flow ratio of the slurry containing microbubbles to phosphoric acid is 30:1. The slurry after the acidolysis reaction is filtered to obtain phosphoric acid and phosphogypsum.

[0093] That is, compared with Example 1, the method does not add active silicon additive in step (1), does not perform the microbubble generation treatment in step (2), and performs microbubble treatment in the acid hydrolysis reaction in step (3). The other conditions are the same as those in Example 1.

[0094] Comparative Example 2

[0095] This comparative example provides a method for enhancing the separation and recovery of fluorine in phosphate ore by using microbubbles.

[0096] The phosphate rock used is the same as that in Example 1.

[0097] The method comprises the following steps:

[0098] (1) Phosphate rock, P 2 O 5Phosphoric acid with a content of 45% and diatomaceous earth as an active silicon auxiliary are mixed for reaction, wherein the mass ratio of phosphate rock to phosphoric acid is 1:1.8, the mass ratio of diatomaceous earth to phosphate rock according to the mass of silicon to the mass of fluorine is 1.5:1, the reaction temperature is 110° C., the reaction time is 3 hours, and a slurry is obtained after the reaction is completed;

[0099] (2) The slurry obtained in step (1) is mixed with sulfuric acid for acid hydrolysis reaction, the mass ratio of sulfuric acid to phosphate rock is 1.1:1, and the P content in the slurry is controlled by adding process water. 2 O 5 The content is 28%, the temperature of the acidolysis reaction is 85°C, the slurry obtained after the acidolysis reaction is used as the water source, and the air is used as the gas source. The gas source and the water source enter the microbubble generating device according to the volume ratio of 1:7, and microbubbles are formed in the slurry. The average diameter of the microbubbles is 500μm. The slurry containing microbubbles is circulated back to the acidolysis reaction. The mass flow ratio of the slurry containing microbubbles to phosphoric acid is 30:1. The slurry after the acidolysis reaction is filtered to obtain phosphoric acid and phosphogypsum.

[0100] That is, compared with Example 1, the method does not perform the microbubble generation treatment in step (2), and performs microbubble treatment in the acid hydrolysis reaction in step (3), and the other conditions are the same as those in Example 1.

[0101] Comparative Example 3

[0102] This comparative example provides a method for enhancing the separation and recovery of fluorine in phosphate ore by using microbubbles.

[0103] The phosphate rock used is the same as that in Example 1.

[0104] The method comprises the following steps:

[0105] (1) Phosphate rock, P 2 O 5 Phosphoric acid with a content of 45% is mixed for reaction, wherein the mass ratio of phosphate rock to phosphoric acid is 1:1.8, the reaction temperature is 110°C, the reaction time is 3h, and a slurry is obtained after the reaction is completed;

[0106] (2) The slurry obtained in step (1) is mixed with sulfuric acid for acid hydrolysis reaction, the mass ratio of sulfuric acid to phosphate rock is 1.1:1, and the P content in the slurry is controlled by adding process water. 2 O 5 The content is 28%, the temperature of the acid hydrolysis reaction is 85°C, and the slurry after the acid hydrolysis reaction is filtered to obtain phosphoric acid and phosphogypsum;

[0107] (3) The phosphoric acid filtered in step (2) is mixed with diatomaceous earth as an active silicon auxiliary agent for reaction, wherein the ratio of the mass of silicon to the mass of fluorine in the diatomaceous earth and the phosphoric acid is 1.5:1, the reaction temperature is 110° C., the reaction time is 3 h, and the phosphoric acid is used as a water source and the air is used as a gas source. The volume ratio of the gas source to the water source is 1:7, and the phosphoric acid and the air enter the microbubble generating device respectively to form microbubbles in the phosphoric acid. The average diameter of the microbubbles is 500 μm. The acid solution containing the microbubbles is circulated back into the phosphoric acid. The mass flow ratio of the acid solution containing the microbubbles to the phosphoric acid is 30:1.

[0108] That is, compared with Example 1, the method does not add active silicon additives in step (1), does not perform the microbubble generation treatment in step (2), adds active silicon additives to the phosphoric acid obtained by filtration in the acid hydrolysis reaction in step (3), and performs microbubble treatment, and the remaining conditions are the same as those in Example 1.

[0109] Comparative Example 4

[0110] This comparative example provides a method for enhancing the separation and recovery of fluorine in phosphate rock by using microbubbles. Compared with Example 1, no active silicon auxiliary agent is added in step (1), and the rest is the same as Example 1.

[0111] Comparative Example 5

[0112] This comparative example provides a method for strengthening the separation and recovery of fluorine in phosphate ore by using a silicon additive. Compared with Example 1, the microbubble generation treatment in step (2) is not performed, and the rest is the same as Example 1.

[0113] Comparative Example 6

[0114] This comparative example provides a method for enhancing the separation and recovery of fluorine in phosphate ore by using bubbles. Compared with Example 1, the microbubble generating device in step (2) is replaced by a bubbling device, that is, an equal amount of gas is used for bubbling, and the average bubble diameter is 2 mm. The rest is the same as Example 1.

[0115] Comparative Example 7

[0116] This comparative example provides a method for enhancing the separation and recovery of fluorine in phosphate ore by steam stripping. Compared with Example 1, the microbubble generating device in step (2) is replaced by a steam stripping device, that is, an equal amount of steam is used as a gas source for steam stripping. The steam pressure of the steam stripping is 0.4 MPa, and the rest is the same as Example 1.

[0117] Performance Characterization

[0118] The fluorine content in the phosphoric acid and phosphogypsum obtained in the examples and comparative examples was measured, and the fluorine recovery rate was calculated. The results are listed in Table 1.

[0119] The fluorine content in phosphoric acid is measured according to "GB / T 21057-2007 General method for determination of fluorine content in inorganic chemical products - ion selective electrode method".

[0120] The fluorine content in phosphate rock and phosphogypsum was detected by X-ray fluorescence spectrometer.

[0121] The calculation method of fluorine recovery rate is as follows:

[0122] Fluorine recovery rate = (mass of phosphate rock * fluorine content of phosphate rock - mass of phosphogypsum * fluorine content in phosphogypsum - mass of phosphoric acid * fluorine content in phosphoric acid) / (mass of phosphate rock * fluorine content of phosphate rock) × 100%

[0123] Table 1

[0124]

[0125] As can be seen from Table 1, the method for fluorine separation and recovery provided by the present invention is aimed at the reaction process of phosphate rock and phosphoric acid, and uses active silicon additives coupled with microbubbles to enhance defluorination, convert fluorine into volatile fluorides, achieve effective defluorination in the wet phosphoric acid process, improve the fluorine recovery rate, and reduce fluorine entrainment in the phosphogypsum product. In Examples 1-3, the fluorine recovery rate is above 98.8%, and no fluorine content is detected in the phosphogypsum.

[0126] Compared with Example 1, in Example 4, the reaction temperature is too low, and fluorosilicic acid is more easily decomposed under high temperature and strong acid conditions. Therefore, the rate at which fluorosilicic acid decomposes into silicon tetrafluoride and hydrogen fluoride is slow, which reduces the fluorine recovery rate; in Example 5, the reaction temperature is too high, resulting in a decrease in gas solubility, and microbubbles are difficult to maintain and easy to agglomerate. Although the rate at which fluorosilicic acid decomposes into silicon tetrafluoride and hydrogen fluoride is accelerated, the lack of microbubble gas "carries it out", which reduces the fluorine recovery rate; in Example 6, the acid solution is weakly acidic, and the rate at which silicic acid decomposes into silicon tetrafluoride and hydrogen fluoride is slow, which reduces the fluorine recovery rate; in Example 7, the acid solution is too acidic, and impurity minerals (calcium feldspar, potassium feldspar, sodium feldspar, pyrite, etc.) will release more impurities such as silicon, aluminum, potassium, sodium, and iron, converting fluorosilicic acid into fluorosilicates and fluoroaluminates and precipitating them, which reduces the fluorine recovery rate and the fluorine content of phosphogypsum is high.

[0127] In Comparative Example 1, microbubble treatment was introduced during sulfuric acid acid hydrolysis, which had a certain defluorination effect. No fluorine content was detected in the phosphogypsum, but fluorine remained in the phosphoric acid product in the form of fluoroaluminates and fluorosilicates, and could not be recovered by microbubbles, resulting in a lower overall fluorine recovery rate; in Comparative Example 2, an active silicon additive was added during the phosphoric acid reaction to convert hydrofluoric acid into fluorosilicic acid, but no microbubble treatment was performed, and the fluoride could not be volatilized and escaped, and then a large amount of fluorosilicic acid was converted into fluorosilicates and fluoroaluminates. The introduction of microbubbles during sulfuric acid acid hydrolysis could not achieve the decomposition and conversion of fluorine, resulting in a low fluorine recovery rate and a high fluorine content in the phosphogypsum; in Comparative Example 3, a silicon additive was added to phosphoric acid and microbubbles were introduced. The fluorine in the phosphoric acid mainly existed in the form of fluorosilicates, fluoroaluminates and a small amount of hydrofluoric acid, which were difficult to convert and decompose, resulting in a low fluorine recovery rate. The fluorine content of gypsum is relatively high; in Comparative Example 4, only microbubble treatment is performed, and fluorine still exists in the form of hydrofluoric acid, and the boiling point of hydrofluoric acid is higher than that of silicon tetrafluoride, and its volatility is weaker than that of silicon tetrafluoride, so it is difficult to take out a large amount of fluorine; in Comparative Example 5, only silicon additive is added, and fluorine is converted from hydrofluoric acid to fluorosilicic acid, but due to the lack of microbubbles, the decomposition rate of fluorosilicic acid is low and it is difficult to volatilize, resulting in a low fluorine recovery rate; in Comparative Example 6, bubbling defluorination is adopted, the gas mass transfer rate is slow, and the existence time of bubbles in the liquid phase is also short, so the amount of gas entering the liquid phase is small, and the fluorine-containing gas cannot be "taken out" quickly, and the microbubbles do not have the ability to decompose fluorosilicic acid, resulting in a low fluorine recovery rate; in Comparative Example 7, steam stripping is adopted, and the acid concentration is reduced due to steam condensation, so that the rate of decomposition of fluorosilicic acid into silicon tetrafluoride and hydrogen fluoride is low, resulting in a low fluorine recovery rate.

[0128] In summary, the method provided by the present invention utilizes the synergistic effect of microbubbles and active silicon additives in the phosphoric acid hydrolysis of phosphate rock to enhance the conversion of fluorine impurities in the phosphate rock into volatile fluoride SiF 4 The fluorine impurities can be separated from the acid hydrolysis source of phosphate rock to avoid fluorine from entering the subsequent wet phosphoric acid process.

[0129] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for strengthening the separation and recovery of fluorine in phosphate ore by using microbubbles coupled with silicon additives, characterized in that: The method comprises the following steps: (1) mixing phosphate rock, phosphoric acid and active silicon additive to react to obtain slurry, and subjecting the slurry to microbubble generation treatment to obtain microbubble slurry, wherein the microbubble slurry is circulated back to the reaction to recover the escaped volatile fluoride, and after the reaction is completed, a defluorinated slurry is obtained; The P2O5 content in the phosphoric acid is 35-55%; The reaction temperature is 95-115°C; The mass ratio of silicon in the active silicon additive to fluorine in the phosphate rock is (0.5-3):1; The gas-liquid volume ratio of the microbubble generation treatment is 1:(5-10); The gas used in the microbubble generation process includes any one of air, N2, O2 or CO2, or a combination of at least two of them; The average diameter of the microbubbles is 300-800 μm; (2) The defluorinated slurry obtained in step (1) is subjected to acid hydrolysis and solid-liquid separation to obtain phosphoric acid and phosphogypsum.

2. The method according to claim 1, characterized in that The composition of the phosphate rock includes: P2O5 15-35wt%, F1.5-4wt%, SiO2 5-15wt%, Al2O3 1-8wt%, Fe2O3 0.1-2wt%, K2O 0.1-3wt%, and Na2O 0.05-1.5wt%.

3. The method according to claim 1, characterized in that The mass ratio of the phosphate rock to the phosphoric acid is 1:(1-2).

4. The method according to claim 1, characterized in that The active silicon auxiliary agent includes any one of diatomaceous earth, white carbon black, silicon powder, silicon dioxide aerogel or nano silicon dioxide, or a combination of at least two thereof.

5. The method according to claim 1, characterized in that: The reaction time in step (1) is 1-5 h.

6. The method according to claim 1, characterized in that During the circulation of the microbubble slurry, the mass flow ratio of the microbubble slurry to phosphoric acid is (20-40):

1.

7. The method according to claim 1, characterized in that The acidolysis reaction comprises reacting the defluorinated slurry with sulfuric acid; The temperature of the acid hydrolysis reaction is 80-105°C; The mass ratio of sulfuric acid to phosphate rock is (0.6-1.4):1; The slurry obtained by the acid hydrolysis reaction is processed with process water to control the P2O5 content in the slurry to be 25-40%.

8. The method according to claim 1, characterized in that The method comprises the following steps: (1) Phosphate rock, phosphoric acid and active silicon additive are mixed and reacted at 95-115° C., wherein the content of P2O5 in the phosphate rock is 15-35wt%, the content of F is 1.5-4wt%, the content of SiO2 is 5-15wt%, the content of Al2O3 is 1-8wt%, the content of Fe2O3 is 0.1-2wt%, the content of K2O is 0.1-3wt%, the content of Na2O is 0.05-1.5wt%, the content of P2O5 in phosphoric acid is 35-55%, the mass ratio of phosphate rock to phosphoric acid is 1:(1-2), and the mass ratio of silicon in the active silicon additive to fluorine in the phosphate rock is (0.5-3):1, to obtain a slurry; and subjecting the slurry to a microbubble generation treatment, wherein the gas-liquid volume ratio in the microbubble generation treatment is 1:(5-10), and the average diameter of the microbubbles is 300-800 μm, to obtain a microbubble slurry; The microbubble slurry is circulated back to the reaction, the flow ratio of the microbubble slurry to phosphoric acid is (20-40):1, and volatile fluoride escapes at the same time, and the fluorine content in the volatile fluoride is 1-12kg / m 3 , volatile fluoride is absorbed by spraying with aqueous solution; The reaction time is 1-5 hours, and a defluorination slurry is obtained after the reaction is completed; (2) The defluorination slurry in step (1) is subjected to an acid hydrolysis reaction with sulfuric acid at 80-105° C., and the mass ratio of sulfuric acid to phosphate rock is (0.6-1.4):

1. After the acid hydrolysis reaction, a slurry is obtained, and the P2O5 content in the slurry is controlled to be 25-40% by adding process water. Then, solid-liquid separation is performed to obtain phosphoric acid and phosphogypsum, and part of the phosphoric acid is returned to the reaction in step (1).