A method for preparing ammonium paratungstate

By adding pyrosulfate roasting and dilute acid leaching treatment to tungsten smelting, combined with the ammonia dissolution-purification and impurity removal-evaporation crystallization process, the high cost and wastewater problems of recycling chromium-containing tungsten oxide waste in the existing technology are solved, and high efficiency is achieved. Preparation of ammonium paratungstate that meets national standards.

CN118637663BActive Publication Date: 2024-10-29CHONGYI ZHANGYUAN TUNGSTEN
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411115032.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-29
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

In the existing tungsten smelting technology, the method of recycling chromium-containing tungsten oxide waste has problems such as long ion exchange process, high production cost, large amount of waste water, etc., making it difficult to effectively prepare ammonium paratungstate products that meet national standards.

Method used

Add pyrosulfate to the chromium-containing tungsten oxide waste for roasting, then leach it with dilute acid and process it through ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate with a chromium content of less than 10 mg/kg.

Benefits of technology

The recycling process is simplified, the production cost is reduced, the amount of waste water is reduced, and the recovery rate of tungsten trioxide is increased, and ammonium paratungstate that meets the national standard zero-grade product is prepared.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of tungsten smelting, and specifically relates to a method for preparing ammonium paratungstate. A certain amount of pyrosulfate is added to chromium-containing tungsten oxide waste for roasting, and the roasted material is leached with dilute acid to remove chromium and other metal impurity ions therein, and the treated tungsten oxide waste is treated by an ammonia solution-purification-impurity removal-evaporation crystallization process to obtain national standard zero-grade ammonium paratungstate (national standard GBT10116-2007 zero-grade product requires that the chromium content in the ammonium paratungstate product is less than 10 mg / kg).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tungsten smelting, and specifically relates to a method for preparing ammonium paratungstate. Background Art

[0002] Since chromium can improve the mechanical properties and corrosion resistance of alloys, it is widely added to cemented carbide. In order to recover tungsten in waste cemented carbide, domestic enterprises generally use electrolysis to separate the bonding phase-cobalt in cemented carbide from tungsten carbide, and then convert tungsten carbide into tungsten oxide waste by high-temperature oxidation. This tungsten oxide waste contains high chromium and other impurities. In order to obtain ammonium paratungstate products with chromium and other impurity contents that meet the requirements of national standard GBT10116-2007, tungsten smelting enterprises usually use sodium hydroxide to alkaline dissolve chromium-containing tungsten oxide waste, and then use ion exchange process to prepare ammonium paratungstate products from chromium-containing sodium tungstate solution. The ion exchange process has the disadvantages of long process flow, high production cost, and large amount of wastewater. Therefore, a more economical and environmentally friendly method for recovering chromium-containing tungsten oxide waste is urgently needed. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a method for preparing ammonium paratungstate.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for preparing ammonium paratungstate comprises the following steps:

[0006] S1. Adding pyrosulfate to the chromium-containing tungsten oxide waste, mixing and then roasting, and cooling to obtain a roasted material;

[0007] S2, leaching the roasted material with dilute acid, filtering and washing, and obtaining tungsten oxide waste;

[0008] S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate, wherein the chromium content in the ammonium paratungstate is less than 10 mg / kg.

[0009] As a preferred embodiment of the method for preparing ammonium paratungstate described in the present invention, in step S1, the amount of pyrosulfate added is 1-5wt% of the mass of the chromium-containing tungsten oxide waste.

[0010] As a preferred embodiment of the method for preparing ammonium paratungstate described in the present invention, wherein: in the step S1, the roasting temperature is 500-700° C., and the roasting time is 0.5-2.0 h.

[0011] As a preferred embodiment of the method for preparing ammonium paratungstate described in the present invention, wherein: in step S1, the pyrosulfate is sodium pyrosulfate or potassium pyrosulfate.

[0012] As a preferred embodiment of the method for preparing ammonium paratungstate described in the present invention, wherein: in the step S2, the concentration of the dilute acid is 3-6wt%, and the dilute acid is dilute sulfuric acid or dilute hydrochloric acid.

[0013] As a preferred embodiment of the method for preparing ammonium paratungstate described in the present invention, wherein: in the step S2, the liquid-to-solid ratio of the dilute acid to the roasting material is (2-4) mL:1 g.

[0014] As a preferred embodiment of the method for preparing ammonium paratungstate described in the present invention, wherein: in the step S2, the leaching temperature is room temperature, and the leaching time is 1 to 3 hours.

[0015] The beneficial effects of the present invention are as follows:

[0016] The invention provides a method for preparing ammonium paratungstate, which comprises the following steps: adding a certain amount of pyrosulfate to chromium-containing tungsten oxide waste material for roasting, leaching chromium and other metal impurity ions therein with dilute acid, and treating the treated tungsten oxide waste material through an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain national standard zero-grade ammonium paratungstate (national standard GBT10116-2007 zero-grade product requires that the chromium content in the ammonium paratungstate product is less than 10 mg / kg). DETAILED DESCRIPTION

[0017] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] The present invention provides a method for preparing ammonium paratungstate, which has the following advantages:

[0019] (1) The present invention has a short production process for recovering chromium-containing tungsten waste, a small amount of wastewater, and a low production cost.

[0020] (2) The present invention can react the chromium-containing compounds in the waste tungsten oxide that are insoluble in acid and alkali with pyrosulfate to produce sodium chromate that is easily soluble in water, thereby effectively removing the chromium element in the waste tungsten material.

[0021] (3) When the present invention uses pyrosulfate to roast the waste tungsten material, a small amount of tungstate will be produced. Using acid to leach the roasted material can not only remove metal impurities in the roasted material, but also reduce the loss of tungsten trioxide. The tungsten trioxide metal recovery rate in the whole process is extremely high.

[0022] According to one aspect of the present invention, the present invention provides the following technical solution:

[0023] A method for preparing ammonium paratungstate comprises the following steps:

[0024] S1. Adding pyrosulfate to the chromium-containing tungsten oxide waste, mixing and then roasting, and cooling to obtain a roasted material;

[0025] S2, leaching the roasted material with dilute acid, filtering and washing, and obtaining tungsten oxide waste;

[0026] S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate, wherein the chromium content in the ammonium paratungstate is less than 10 mg / kg.

[0027] Preferably, in step S1, the amount of pyrosulfate added is 1-5wt% of the mass of the chromium-containing tungsten oxide waste. Specifically, the amount of pyrosulfate added can be, for example, any one of 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt% of the mass of the chromium-containing tungsten oxide waste, or a range between any two thereof.

[0028] Preferably, in step S1, the calcination temperature is 500-700°C, and the calcination time is 0.5-2.0h. Specifically, the calcination temperature can be, for example, any one of 500°C, 550°C, 600°C, 650°C, 700°C, or any range between two thereof.

[0029] Preferably, in step S1, the pyrosulfate is sodium pyrosulfate or potassium pyrosulfate.

[0030] Preferably, in step S2, the concentration of the dilute acid is 3-6wt%, and the dilute acid is dilute sulfuric acid or dilute hydrochloric acid. Specifically, the concentration of the dilute acid can be, for example, any one of 3wt%, 4wt%, 5wt%, 6wt%, or any range between two thereof.

[0031] Preferably, in step S2, the liquid-solid ratio of the dilute acid to the roasting material is (2-4) mL:1 g. Specifically, the liquid-solid ratio of the dilute acid to the roasting material can be, for example, any one of 2 mL:1 g, 2.5 mL:1 g, 3 mL:1 g, 3.5 mL:1 g, 4 mL:1 g, or a range between any two thereof.

[0032] Preferably, in step S2, the leaching temperature is room temperature and the leaching time is 1 to 3 hours.

[0033] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0034] The composition of the chromium-containing tungsten oxide waste treated in each embodiment and comparative example is shown in the following table:

[0035]

[0036] Example 1

[0037] A method for preparing ammonium paratungstate comprises the following steps:

[0038] S1. Add 8 g of sodium pyrosulfate to 200 g of chromium-containing tungsten oxide waste, mix well and then calcine at a temperature of 600° C. for 1.0 h, and obtain a calcined material after cooling;

[0039] S2, leaching 200g of the roasted material with 600mL of 5wt% dilute sulfuric acid at room temperature for 2h, then filtering and washing to obtain tungsten oxide waste;

[0040] S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate. After testing, the chromium content in the ammonium paratungstate prepared in this embodiment is 3 mg / kg.

[0041] Example 2

[0042] A method for preparing ammonium paratungstate comprises the following steps:

[0043] S1. Add 10 g of sodium pyrosulfate to 200 g of chromium-containing tungsten oxide waste, mix well and then calcine at a temperature of 600° C. for 1.0 h, and obtain a calcined material after cooling;

[0044] S2, leaching 200g of the roasted material with 600mL of 6wt% dilute sulfuric acid at room temperature for 2h, then filtering and washing to obtain tungsten oxide waste;

[0045] S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate. After testing, the chromium content in the ammonium paratungstate prepared in this embodiment is 3 mg / kg.

[0046] Example 3

[0047] A method for preparing ammonium paratungstate comprises the following steps:

[0048] S1. Add 8 g of potassium pyrosulfate to 200 g of chromium-containing tungsten oxide waste, mix well and then calcine at a temperature of 700° C. for 2.0 h, and obtain a calcined material after cooling;

[0049] S2, leaching 200g of the roasted material with 600mL of 6wt% dilute hydrochloric acid at room temperature for 2h, then filtering and washing to obtain tungsten oxide waste;

[0050] S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate. After testing, the chromium content in the ammonium paratungstate prepared in this embodiment is 5 mg / kg.

[0051] Example 4

[0052] A method for preparing ammonium paratungstate comprises the following steps:

[0053] S1. Add 8 g of sodium pyrosulfate to 200 g of chromium-containing tungsten oxide waste, mix well and then calcine at a temperature of 500° C. for 2.0 h, and obtain a calcined material after cooling;

[0054] S2, leaching 200g of the roasted material with 800mL of 3wt% dilute sulfuric acid at room temperature for 2h, then filtering and washing to obtain tungsten oxide waste;

[0055] S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate. After testing, the chromium content in the ammonium paratungstate prepared in this embodiment is 4 mg / kg.

[0056] Example 5

[0057] A method for preparing ammonium paratungstate comprises the following steps:

[0058] S1. Add 8 g of sodium pyrosulfate to 200 g of chromium-containing tungsten oxide waste, mix well and then calcine at a temperature of 600° C. for 2.0 h, and cool to obtain a calcined material;

[0059] S2, leaching 200g of the roasted material with 400mL of 5wt% dilute sulfuric acid at room temperature for 3h, then filtering and washing to obtain tungsten oxide waste;

[0060] S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate. After testing, the chromium content in the ammonium paratungstate prepared in this embodiment is 6 mg / kg.

[0061] Example 6

[0062] A method for preparing ammonium paratungstate comprises the following steps:

[0063] S1. Add 2 g of sodium pyrosulfate to 200 g of chromium-containing tungsten oxide waste, mix well and then calcine at a temperature of 600° C. for 1 h, and cool to obtain a calcined material;

[0064] S2, leaching 200g of the roasted material with 400mL of 3wt% dilute sulfuric acid at room temperature for 3h, then filtering and washing to obtain tungsten oxide waste;

[0065] S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate. After testing, the chromium content in the ammonium paratungstate prepared in this comparative example is 9 mg / kg.

[0066] Comparative Example 1

[0067] The difference from Example 1 is that step S1 is not performed, and step S2 is to leach 200g of chromium-containing tungsten oxide waste with 600mL of 5wt% dilute sulfuric acid at room temperature for 2h, followed by filtering and washing to obtain tungsten oxide waste; step S3 is to treat the tungsten oxide waste with an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate. After testing, the chromium content in the ammonium paratungstate prepared in this comparative example is 175mg / kg.

[0068] Comparative Example 2

[0069] The difference from Example 1 is that dilute sulfuric acid with a concentration of 1 wt % is used in step S2.

[0070] After testing, the chromium content in the ammonium paratungstate prepared in this comparative example is 25 mg / kg, and the sodium content is 39 mg / kg (the national standard GBT10116-2007 zero-grade product requires that the sodium and chromium contents in the ammonium paratungstate product are both less than 10 mg / kg).

[0071] Comparative Example 3

[0072] The difference from Example 1 is that water is used instead of dilute sulfuric acid for leaching in step S2.

[0073] After testing, the chromium content in the ammonium paratungstate prepared in this comparative example is 65 mg / kg, and the sodium content is 169 mg / kg (the national standard GBT10116-2007 zero-grade product requires that the sodium and chromium contents in the ammonium paratungstate product are both less than 10 mg / kg).

[0074] Comparative Example 4

[0075] The difference from Example 1 is that step S2 is not performed, and in step S3, the roasted material is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate.

[0076] After testing, the chromium content in the ammonium paratungstate prepared in this comparative example is 175 mg / kg, and the sodium content is 634 mg / kg (the national standard GBT10116-2007 zero-grade product requires that the sodium and chromium contents in the ammonium paratungstate product are both less than 10 mg / kg).

[0077] It can be seen from the above embodiments and comparative examples that the present invention adds a certain amount of pyrosulfate to the chromium-containing tungsten oxide waste material for roasting, and uses dilute acid to leach chromium and other metal impurity ions therein, and the treated tungsten oxide waste material is treated by ammonia dissolution-purification and impurity removal-evaporation and crystallization process to obtain national standard zero-grade ammonium paratungstate (national standard GBT10116-2007 zero-grade product requires that the chromium content in the ammonium paratungstate product is less than 10 mg / kg).

[0078] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing ammonium paratungstate, characterized in that: The steps include: S1. Adding sodium pyrosulfate to the chromium-containing tungsten oxide waste, mixing and then roasting, cooling and obtaining a roasted material, wherein the chromium in the chromium-containing tungsten oxide waste is in the form of Cr2O3; S2, leaching the roasted material with dilute acid, the concentration of the dilute acid is 3-6wt%, the dilute acid is dilute sulfuric acid or dilute hydrochloric acid, and then filtering and washing to obtain tungsten oxide waste; S3. The waste tungsten oxide is treated by an ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain ammonium paratungstate, wherein the chromium content in the ammonium paratungstate is less than 10 mg / kg.

2. The method for preparing ammonium paratungstate according to claim 1, characterized in that: In the step S1, the amount of sodium pyrosulfate added is 1-5wt% of the mass of the chromium-containing tungsten oxide waste.

3. The method for preparing ammonium paratungstate according to claim 1, characterized in that: In the step S1, the calcination temperature is 500-700° C., and the calcination time is 0.5-2.0 h.

4. The method for preparing ammonium paratungstate according to claim 1, characterized in that: In the step S2, the liquid-to-solid ratio of the dilute acid to the roasting material is (2-4) mL:1 g.

5. The method for preparing ammonium paratungstate according to claim 1, characterized in that: In step S2, the leaching temperature is room temperature and the leaching time is 1 to 3 hours.

Citation Information

Patent Citations

  • Analyses testing method of aluminum, calcium, iron, molybdenum, niobium, titanium, tungsten impurity elements in chromium carbide

    CN101303307A

  • Supported type three-center catalyst and preparation method and application thereof

    CN110204636A