A method for preparing high-crystalline high-molecular-weight polyvinylidene fluoride resin

By controlling the batch addition and reaction conditions of the initiator and chain transfer agent in the suspension polymerization reaction, the problem of difficult control of the molecular weight distribution and crystallinity of polyvinylidene fluoride resin in the prior art was solved, and high molecular weight and low dispersion were prepared. , high crystallinity polyvinylidene fluoride resin meets the needs of high-performance materials.

CN118638256BActive Publication Date: 2024-11-08SHANDONG DE YI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105510.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing supercritical suspension polymerization methods are difficult to accurately control the molecular weight distribution and crystallinity of polyvinylidene fluoride resins, and cannot meet the needs of some specific application fields.

Method used

By adding degassing water and dispersant to the reactor, gradually adding vinylidene fluoride after heating, and intermittently adding initiator and chain transfer agent to control the reaction pressure and temperature, and finally quickly transfer to the receiving kettle for cooling and discharge. gas reduces the reaction afterwards, thereby preparing polyvinylidene fluoride resins with high molecular weight, low dispersion and high crystallinity.

Benefits of technology

Accurate control of polymerization reaction is achieved, and the obtained polyvinylidene fluoride resin has a narrower molecular weight distribution and higher crystallinity, meeting the needs of high-performance materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118638256B_ABST
    Figure CN118638256B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polymerization process, and discloses a method for preparing a high-crystalline high-molecular-weight polyvinylidene fluoride resin. In a reactor, degassed water and a dispersant are added, the temperature is started to rise, the oxygen in the reactor is replaced with nitrogen, vinylidene fluoride is added, an initiator and a chain transfer agent are added, and the reaction is started. During the polymerization process, vinylidene fluoride is added to maintain the reactor pressure, and the initiator and the chain transfer agent are intermittently added during the reaction process (initiator: chain transfer agent = 1: 2~5), and the material is quickly transferred to a receiving reactor after the reaction is completed. The addition of the initiator in batches can accurately control the reaction rate. According to the reaction temperature, pressure and other factors, adding an appropriate amount of initiator at a specific point helps to control the amount of primary free radicals in the entire reaction system, can control the polymerization more uniformly in the entire reaction stage, make the molecular weight distribution narrower, help to inhibit side reactions, and prevent the reaction from being terminated prematurely.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymerization technology, in particular to a method for preparing high-crystallization high-molecular weight polyvinylidene fluoride resin. Background Art

[0002] Polyvinylidene fluoride (PVDF) has attracted people's attention since it was first successfully synthesized in 1948. Its repeating unit is , and The alternating arrangement of groups makes PVDF resin have the characteristics of both fluororesin and general resin. In addition to good chemical corrosion resistance, high temperature resistance, oxidation resistance, weather resistance, UV resistance, radiation resistance, it also has special properties such as piezoelectricity and thermoelectricity.

[0003] PVDF has been widely used as a binder, electrolyte and diaphragm material due to its good mechanical properties, electrical properties and chemical stability. PVDF has a regular structure, is easy to crystallize, and has strong adhesion. When used as a binder, it can make the electrode show high mechanical strength. When used in polymer electrolytes, the high mechanical strength can make the polymer chain play the role of skeleton support. At the same time, its high dielectric constant (~10) and electron-repelling group The presence of is conducive to the dissociation of electrolyte salts and provides a higher carrier concentration. In addition, PVDF also has good wettability and good affinity for electrolytes, making it an ideal alternative material for commercial polyolefin separators, which is conducive to the development of energy storage devices towards higher performance.

[0004] These application fields usually require PVDF resins with high molecular weight and low dispersibility. At present, the preparation of high-purity PVDF resin generally adopts the method of suspension polymerization, because compared with emulsion polymerization, the suspension polymerization method can more easily remove various additives used in the reaction, and the purity of the obtained PVDF resin is higher. However, the PVDF resin obtained by the existing supercritical suspension polymerization preparation method cannot achieve precise control of molecular weight distribution and crystallinity, and cannot meet the needs of some specific application fields.

[0005] In the polyvinylidene fluoride suspension polymerization process disclosed in patent CN110229255A, vinylidene fluoride monomer, initiator, dispersant and chain transfer agent are added into a reactor at one time and then the temperature is raised for reaction, which simplifies the reaction process. However, the pressure in the reactor varies greatly from the beginning to the end of the reaction, resulting in a wide molecular weight distribution of the product.

[0006] In the vinylidene fluoride suspension polymerization process in patent CN101072801A, the polymerization reaction temperature and pressure are increased. Before the polymerization reaction, part of the monomer is added to the reactor, and the initiator, dispersant and chain transfer agent are added to the reactor at one time and then the temperature is raised for reaction. The monomer is continuously added during the reaction process to maintain the supercritical reaction pressure. However, this method has a fast initial free radical generation rate and a large number of free radicals, which increases the disproportionation and dehydrogenation side reactions between free radicals. In addition, as the reaction temperature increases, the initiator decays rapidly, resulting in a decrease in the number of subsequent free radicals, a decrease in the reaction rate, and a wide molecular weight distribution of the final product.

[0007] Patent CN101434670A prepares high-crystallinity PVDF. The initiator used is a redox initiator, wherein the oxidant is cumene peroxide and the reductant is uranium hypochlorite. However, the benzene ring structure is difficult to completely remove after treatment, and will cause high-temperature coloration of the PVDF resin.

[0008] Patent CN103146101A heat-treats PVDF resin to control the molecular crystallization process and obtain high-crystallinity PVDF resin. However, this method is complex and physical. The resulting product may have a decreased crystallinity after long-term use. This method cannot fundamentally improve the crystallinity of PVDF resin.

[0009] Patent CN116375915A discloses a suspension polymerization process for preparing long-chain branched high molecular weight polyvinylidene fluoride by adding initiator and chain transfer agent in batches. The patent does not provide a detailed description of the control means of the addition process, and the obtained product has a long-chain branched structure.

[0010] In the prior art, after the reaction reaches a certain level, the feeding is stopped and the unreacted monomer is discharged from the reactor. After the pressure of the system is reduced, the material is discharged for post-processing. However, since the PVDF in the supercritical suspension polymerization reactor is operated at a full liquid level, the exhaust is too fast and the material is easily carried out. The exhaust process is slow and the exhaust time is long. During this process, the reaction is not completely stopped, and the molecular weight distribution of the obtained product is wide.

[0011] The present invention further develops a suspension polymerization method capable of preparing high molecular weight, low dispersibility and high crystallinity PVDF resin. Summary of the invention

[0012] Based on the above content, the present invention provides a method for controlling the decomposition amount of an initiator to prepare a polyvinylidene fluoride resin with high molecular weight, narrow molecular weight distribution and high crystallinity.

[0013] The method is as follows:

[0014] In the reactor, deaerated water and dispersant are added, the temperature begins to rise, the oxygen in the reactor is replaced with nitrogen, vinylidene fluoride is added, initiator and chain transfer agent are added, and the reaction begins. During the polymerization process, vinylidene fluoride is added to maintain the reactor pressure. During the reaction process, initiator and chain transfer agent are intermittently added (initiator: chain transfer agent = 1:2~5 (W / W)). After the reaction is completed, the material is quickly transferred to the receiving reactor, the pressure is quickly reduced and the temperature is lowered, and the exhaust is performed to reduce the post-reaction in the cooling and exhausting stages, so as to obtain a high molecular weight, low dispersity polyvinylidene fluoride resin.

[0015] Before the polymerization reaction begins, an initiator accounting for 0.01-0.1 wt% of the degassed water is added to the reactor, and then the decomposed initiator is added back to the reaction system according to the decomposition rate of the initiator. The initiator can be added intermittently or continuously according to the dosage, preferably continuously.

[0016] The initiator of suspension polymerization is one or more of diethyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, tert-butyl peroxypivalate, tert-butyl peroxide, di-tert-amyl peroxide, ethyl-tert-butyl peroxide, tert-butyl peroxypivalate, and ammonium persulfate. The initiator is added before the reaction starts, accounting for 0.01-0.1 wt% of the amount of degassed water added.

[0017] Before the polymerization reaction begins, 0.02-0.4 wt% of the chain transfer agent, which accounts for 0.02-0.4 wt% of the degassed water, is added into the reactor. The amount of the chain transfer agent added is 1-5 times the mass of the initiator, preferably 2-4 times.

[0018] The chain transfer agent for suspension polymerization is one or more of ethyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, diethyl malonate, isopropyl ketone, methyl propionate, ethyl propionate, and diethyl succinate. The amount of the chain transfer agent added before the reaction starts is 2 to 4 times the mass of the initiator added.

[0019] The amount of chain transfer agent added after the reaction starts is 2 to 4 times the mass of the initiator. The chain transfer agent can be added together with the initiator or added separately. Preferably, it is mixed with the initiator in proportion and added together.

[0020] The suspension polymerization reaction temperature is 45~55℃.

[0021] The suspension polymerization reaction pressure is 6.5~8Mpa.

[0022] The dispersant for suspension polymerization is one or two of methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, hydroxyethyl methyl ethyl cellulose and polyvinyl alcohol.

[0023] After the feeding of vinylidene fluoride was stopped, the reaction in the kettle continued for 2 hours, during which time no initiator and chain transfer agent were added.

[0024] After the reaction is finished, the material in the reactor is quickly pressed into the receiving reactor through the bottom valve, so that the entire system is quickly depressurized and cooled, thereby achieving the purpose of quickly stopping the reaction. Among them, the receiving reactor is 0.5 to 10 times the volume of the reactor, preferably 1 to 5 times, and most preferably 2 to 5 times. And the receiving reactor can be cooled with a jacket or without a jacket, preferably with a jacket, and the temperature of the condensed water in the jacket is 0 to 50°C, and conventional room temperature water is more preferably used.

[0025] The unreacted gas in the receiving kettle and the reactor is discharged to the waste gas recovery system. After the gas is emptied, the polyvinylidene fluoride in the receiving kettle is washed with 70°C hot water for multiple times, and the washed PVDF resin is dried at 120°C for 6 hours.

[0026] The present invention has the following beneficial effects:

[0027] Adding the initiator in batches can precisely control the reaction rate. Adding the appropriate amount of initiator at a specific point based on the reaction temperature, pressure and other factors helps control the amount of primary free radicals in the entire reaction system, which can control a more uniform polymerization throughout the reaction stage, making the molecular weight distribution narrower, helping to inhibit side reactions and prevent premature termination of the reaction.

[0028] The polymerization of vinylidene fluoride is an exothermic reaction. In the exothermic polymerization reaction, the addition of initiator in batches can more effectively control the heat of generation. The reaction rate is controlled to be stable, the risk of overheating and thermal runaway is reduced, and safety and product quality are ensured. In the present invention, when the process control step has a large deviation, the initiator content in the reactor can be theoretically calculated based on the initial initiator amount added and the additional initiator amount and addition time, and then the initiator addition speed is adjusted in real time through automatic control to ensure the stability of the initiator concentration in the reaction system as much as possible.

[0029] The chain transfer agent is added in batches, and its concentration can be precisely adjusted during the polymerization, which can better control the molecular weight of the polymer. In some polymerization processes, excessive chain transfer agent will lead to reaction termination, crosslinking and gel formation. The chain transfer agent is added in batches to reduce the excessive amount of small molecular weight products caused by excessive initial one-time addition and premature termination of the reaction; and minimize the risk of undesirable crosslinking. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention is further described in detail below with reference to the accompanying drawings and specific implementation methods.

[0031] Figure 1 Block flow diagram for suspension polymerization. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The analysis methods in the embodiments and comparative examples are as follows:

[0034] 1) Molecular weight analysis method

[0035] The weight average molecular weight (Mw) was used for characterization. Specifically, the test was carried out by gel permeation chromatography. The test conditions were: dimethylformamide (DMF) containing 0.1% lithium bromide was used as the eluent, the differential refractive index RI was used as the detector, the polystyrene calibration reagent was used as the standard, the test temperature was 40°C, and the flow rate was 1.0 mL / min.

[0036] 2) Melting temperature and crystallinity analysis method

[0037] The DSC test was performed in a N atmosphere using a differential scanning calorimeter (DSC, Mettler-Toledo). The temperature was raised to 200°C at a rate of 10°C / min and kept constant for 10 min to eliminate the thermal history. The temperature was lowered to -80°C at the same rate and then raised at the same rate to determine the melting behavior. The area of ​​the crystal melting exothermic peak is closely related to the crystallinity. The melting enthalpy was calculated based on the melting peak area of ​​the heating DSC curve. ,

[0038] The crystallinity calculation formula of polymer is as follows:

[0039] .

[0040] in is the melting enthalpy of the test sample, is the thermal enthalpy of complete crystallization of polyvinylidene fluoride. .

[0041] Embodiment 1

[0042] Add 19.5 kg of degassed water and 7.5 g of methylcellulose to a 30 L autoclave, start stirring the reactor, heat the reactor to 50 °C, evacuate, and replace with nitrogen several times until the oxygen content in the reactor is less than 20 ppm. Add vinylidene fluoride until the pressure in the reactor is 7.2 MPa, use a high-pressure pump to add 6 g of diisopropyl peroxydicarbonate and 18 g of isopropyl alcohol to start the reaction, and when the pressure in the reactor reaches 7.1 MPa, start adding vinylidene fluoride, and at the same time, add initiator and chain transfer agent at a rate of 0.12 g of diisopropyl peroxydicarbonate and 0.3 g of isopropyl alcohol per minute. When the total feed amount of vinylidene fluoride reaches 11.4 kg, stop adding vinylidene fluoride. 2 hours after the feed of vinylidene fluoride stops, stop the reaction, discharge the materials in the reactor into the receiving reactor through the bottom valve, and discharge the unreacted gas in the reactor and the receiving reactor to the waste gas recovery system. Wash and dry the suspension obtained by polymerization with hot water.

[0043] Embodiment 2

[0044] Add 19.5 kg of deaerated water and 7.5 g of methylcellulose to a 30L autoclave, start stirring the reactor, heat the reactor to 50 °C, evacuate, and replace with nitrogen several times until the oxygen content in the reactor is less than 20 ppm. Add vinylidene fluoride until the pressure in the reactor is 7.2 MPa, use a high-pressure pump to add 6 g of diisopropyl peroxydicarbonate and 18 g of isopropanol as initiator, start the reaction, and start adding vinylidene fluoride when the pressure in the reactor reaches 7.1 MPa. After the pressure drops, after 40 minutes of reaction, add 1.8 g of initiator and 9 g of isopropanol every 30 minutes for 2 times. When the total amount of vinylidene fluoride feed reaches 11.4 kg, stop adding vinylidene fluoride. 2 hours after the vinylidene fluoride feed stops, stop the reaction, discharge the material in the reactor into the receiving reactor through the bottom valve, and discharge the unreacted gas in the reactor and the receiving reactor to the waste gas recovery system. Wash and dry the suspension obtained by polymerization with hot water.

[0045] Embodiment 3

[0046] Add 19.5 kg of degassed water and 7.5 g of methylcellulose to a 30 L autoclave, start stirring the reactor, heat the reactor to 50 °C, evacuate, and replace with nitrogen several times until the oxygen content in the reactor is less than 20 ppm. Add vinylidene fluoride until the pressure in the reactor is 7.2 MPa, use a high-pressure pump to add 6 g of diisopropyl peroxydicarbonate and 12 g of isopropyl alcohol as initiator, start the reaction, and when the pressure in the reactor reaches 7.1 MPa, start adding vinylidene fluoride. After the pressure starts to drop, add 3 g of diisopropyl peroxydicarbonate and 3 g of isopropyl alcohol every 45 minutes. When the total amount of vinylidene fluoride feed reaches 11.4 kg, stop adding vinylidene fluoride. 2 hours after vinylidene fluoride stops feeding, stop the reaction, discharge the material in the reactor into the receiving reactor through the bottom valve, and discharge the unreacted gas in the reactor and the receiving reactor to the waste gas recovery system. Wash the suspension obtained by polymerization with hot water and dry it.

[0047] Embodiment 4

[0048] Into a 30 L autoclave, add 19.5 kg of degassed water and 7.5 g of methylcellulose, start the reactor and stir, heat the reactor to 50 °C, evacuate, and replace with nitrogen several times until the oxygen content in the reactor is less than 20 ppm. Add vinylidene fluoride until the pressure in the reactor is 7.2 MPa, use a high-pressure pump to add 6 g of diisopropyl peroxydicarbonate and 6 g of isopropanol as initiator, start the reaction, and when the pressure in the reactor reaches 7.1 MPa, start adding vinylidene fluoride. After the pressure starts to drop, add 3 g of diisopropyl peroxydicarbonate and 3 g of isopropanol for every 1.5 kg of vinylidene fluoride added. When the total amount of vinylidene fluoride fed reaches 11.4 kg, stop adding vinylidene fluoride. 2 hours after the vinylidene fluoride feed stops, stop the reaction, discharge the materials in the reactor into the receiving reactor, and discharge the unreacted gas in the reactor and the receiving reactor to the exhaust system. Wash the suspension obtained by polymerization with hot water and dry it.

[0049] Comparative Example 1

[0050] Into a 30 L autoclave, add 19.5 kg of degassed water and 7.5 g of methylcellulose, start the reactor and stir, heat the reactor to 50 °C, evacuate, and replace with nitrogen several times until the oxygen content in the reactor is less than 20 ppm. Add vinylidene fluoride until the pressure in the reactor is 7.2 MPa, use a high-pressure pump to add 12 g of diisopropyl peroxydicarbonate and 18 g of isopropanol as initiator, start the reaction, and when the pressure in the reactor reaches 7.1 MPa, start adding vinylidene fluoride. When the total amount of vinylidene fluoride feed reaches 11.4 kg, stop adding vinylidene fluoride. 2 hours after the vinylidene fluoride feed stops, stop the reaction, discharge the materials in the reactor into the receiving reactor, and discharge the unreacted gas in the reactor and the receiving reactor to the exhaust system. Wash the suspension obtained by polymerization with hot water and dry it.

[0051] Comparative Example 2

[0052] Add 19.5 kg of degassed water and 7.5 g of methylcellulose to a 30 L autoclave, start the autoclave and stir, heat the autoclave to 50 °C, evacuate, and replace with nitrogen several times until the oxygen content in the autoclave is less than 20 ppm. Add vinylidene fluoride until the pressure in the autoclave is 7.2 MPa, use a high-pressure pump to add 3 g of diisopropyl peroxydicarbonate and 18 g of isopropyl alcohol as initiator, start the reaction, and when the pressure in the autoclave reaches 7.1 MPa, start adding vinylidene fluoride. After the reaction starts, add 3 g of diisopropyl peroxydicarbonate and 9 g of isopropyl alcohol every 60 min. When the total amount of vinylidene fluoride fed reaches 11.4 g, stop adding vinylidene fluoride. 2 hours after the vinylidene fluoride feed stops, stop the reaction, discharge the unreacted gas in the autoclave to the exhaust system, open the autoclave, and wash and dry the suspension obtained by polymerization with hot water.

[0053] The polyvinylidene fluoride resins prepared in Examples 1-4 and Comparative Examples 1-2 were sampled and analyzed, and the results are shown in Table 1.

[0054] Table 1 Sampling and analysis results of polyvinylidene fluoride resin prepared in Example and Comparative Example

[0055]

[0056] As can be seen from Table 1, the polyvinylidene fluoride resin obtained by this method has higher crystallinity, higher melting point and smaller molecular weight dispersion index.

[0057] Of course, it is obvious that the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For those of ordinary skill in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all implementation methods here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a high-crystalline high-molecular-weight polyvinylidene fluoride resin, characterized in that: The following steps are involved: S1. Add degassed water and dispersant to the reactor, start heating, replace oxygen in the reactor with nitrogen, add vinylidene fluoride, initiator and chain transfer agent, start reaction, and carry out polymerization reaction under the conditions of reactor pressure 6.5~8.0Mpa and temperature 45~55℃; S2. Add vinylidene fluoride to maintain the autoclave pressure during the polymerization process, and add initiator and chain transfer agent during the reaction; S3, after the reaction is finished, the material is quickly transferred to the receiving kettle, the pressure is quickly reduced, the temperature is quickly reduced, and the exhaust is performed to reduce the post-reaction in the cooling and exhausting stage, so as to obtain a high molecular weight, low dispersibility polyvinylidene fluoride resin; Before the polymerization reaction begins, 0.01-0.1wt% initiator and 0.02-0.4wt% chain transfer agent are added to the reactor according to the decomposition rate of the initiator, and then the decomposed initiator is added back to the reaction system according to the decomposition rate of the initiator; the initiator and the chain transfer agent are added in batches, and the addition process of the initiator and the chain transfer agent is controlled. When the reaction stops, the initiator and the chain transfer agent are transferred to the receiving reactor, and the pressure and temperature in the reactor are quickly reduced, and the unreacted monomers are discharged, so as to control the molecular weight of the polyvinylidene fluoride, reduce the dispersibility, and improve the crystallinity of the polyvinylidene fluoride resin; During the polymerization reaction, the remaining initiator and chain transfer agent are added continuously or in batches, and the amount of chain transfer agent added is 2 to 4 times the amount of initiator added; When the W / W ratio of the added amount of vinylidene fluoride monomer to the total amount of water reaches (33~50): (50~67), stop feeding vinylidene fluoride, and when the kettle pressure drops to 3~5Mpa, stop the reaction.

2. The method for preparing a high-crystalline high-molecular-weight polyvinylidene fluoride resin according to claim 1, characterized in that: The volume of the receiving kettle is 1~5 times the volume of the reaction kettle. The receiving kettle is equipped with a jacket for cooling, and the temperature of the condensed water in the jacket is 0~50℃.

3. The method for preparing a high-crystalline high-molecular-weight polyvinylidene fluoride resin according to claim 1, characterized in that: The molecular weight of polyvinylidene fluoride (PVDF) is 80~300w, the dispersion number is 1~3, and the crystallinity is 45~60%.

4. The method for preparing a high-crystalline high-molecular-weight polyvinylidene fluoride resin according to claim 1, characterized in that: Before the polymerization reaction begins, an initiator is added at 0.01-0.1 wt% of the amount of deoxygenated water, and a chain transfer agent is added at 200-400 wt% of the amount of initiator.

5. The method for preparing a high-crystalline high-molecular-weight polyvinylidene fluoride resin according to claim 1, characterized in that: The dispersant is methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, hydroxyethyl methyl ethyl cellulose, polypropylene alcohol; The initiator is diethyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, tert-butyl peroxypivalate, tert-butyl peroxide, di-tert-amyl peroxide, ethyl-tert-butyl peroxide, tert-butyl peroxypivalate, and ammonium persulfate; The chain transfer agent is ethyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, diethyl malonate, isopropyl ketone, methyl propionate, ethyl propionate, and diethyl succinate.

6. The method for preparing a high-crystalline high-molecular-weight polyvinylidene fluoride resin according to claim 1, characterized in that: In step S2, the ratio of initiator to chain transfer agent W / W is 1:2-5.