A preparation process of environmentally friendly black ink

By introducing modified monomer blocks and sulfur-nitrogen structures into the water-based binder, the metallic black pigment is stably dispersed, solving the problem of insufficient dispersion of the inorganic black colorant and preparing an environmentally friendly black ink with high stability and excellent printing quality. .

CN118638447BActive Publication Date: 2024-10-18JIANGXI GUCHUAN TAPE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411123016.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-18
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The dispersion stability of the inorganic black colorant in the water-based resin binder is insufficient, which increases the difficulty of construction and affects the printing quality.

Method used

Metallic black pigment, covering agent, wetting agent, leveling agent and distilled water are premixed, then a self-made modified water-based binder is added for grinding and dispersion, and mixed with a drier to prepare environmentally friendly black ink. The modified monomer is embedded in Section introduces sulfur and nitrogen structures into the macromolecular polymer chain to stably disperse the black pigment.

Benefits of technology

The preparation of water-dispersible black ink is realized, which significantly improves the dispersion stability of the pigment and the color stiffness of the printing layer. The ink has excellent stability, is easy to construct, and improves the printing quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a preparation process of an environmentally friendly black ink, and belongs to the technical field of ink. The raw materials of the ink include: 16-21wt% of metallic black pigment, 1.8-2.2wt% of covering agent, 0.25-0.3wt% of wetting agent, 0.1-0.15wt% of leveling agent, 0.12-0.18wt% of defoamer, 1.3-1.6wt% of drying agent and 26-31wt% of distilled water, and the remainder is an aqueous vehicle; wherein the aqueous vehicle has good compatibility with common black pigments such as black iron oxide, black manganese iron and copper chromium black, and the sulfur-nitrogen structure in its structure has a complexation with the pigment, and the pigment is carried for dispersion, so that the stability of the ink is excellent, and at the same time, a cyclosiloxane structure block is introduced to break the uniform chain structure of the polymer, and the multi-level structure of the in-situ complexation enrichment pigment is made so that the color of the printing layer is high, the glossiness is moderate, and the human eye is more comfortable to observe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inks, and in particular relates to a preparation process of environmentally friendly black ink. Background Art

[0002] Ink is a substance used to form graphic information during the printing process. It directly determines the tone, color, and clarity of the image on the printed product, so it plays a huge role in the printing process. Generally, printing ink is mainly composed of binders, colorants, and other additives.

[0003] The binder is a viscous fluid that acts as a carrier for the colorant. Its main function is to bond the colorant to form a film. Existing binders are mostly based on polymer resins, such as common polyurethane, epoxy resin, acrylic resin, etc. Traditional resin binders are mostly dissolved in solvent oil. With the improvement of environmental protection requirements and people's environmental awareness, inks are gradually developing towards water-based. Among them, water-based acrylic resins have good film-forming adhesion and high designability of molecular chain structure, and are widely used in water-based inks.

[0004] Colorants are pigments, which are the coloring materials of inks and directly determine the printing coloring effect of inks. Colorants are mainly divided into two categories according to their types: organic colorants and inorganic colorants. Among them, inorganic black pigments are widely used in various black inks because of their wide sources, low cost and stable coloring effect. However, the dispersion stability of inorganic black colorants in water-based resin binders is insufficient, which increases the difficulty of construction and has a great impact on printing quality. Summary of the invention

[0005] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a preparation process of environmentally friendly black ink.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A preparation process of an environmentally friendly black ink comprises the following steps: premixing a metallic black pigment, a covering agent, a wetting agent, a leveling agent and distilled water, adding an aqueous connecting material, grinding and dispersing the mixture, filtering the mixture, and then adding a drying agent and mixing the mixture to obtain the environmentally friendly black ink.

[0008] Furthermore, the proportions of each raw material in the environmentally friendly black ink are: metallic black pigment 16-21wt%, concealing agent 1.8-2.2wt%, wetting agent 0.25-0.3wt%, leveling agent 0.1-0.15wt%, defoaming agent 0.12-0.18wt%, drying agent 1.3-1.6wt% and distilled water 26-31wt%, and the balance is water-based binder.

[0009] Further, the metallic black pigment includes one of iron oxide black, manganese iron black and copper chrome black.

[0010] Furthermore, the covering agent is hydrophilic titanium dioxide.

[0011] The aqueous vehicle is prepared by the following method:

[0012] Step A1: Dissolve β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol under nitrogen protection, add tetramethyltetravinylcyclotetrasiloxane and mix well, heat to 65-75°C, and heat with 180-260W / m 2 UV irradiation, stirring and reflux for 2.5-3.5h, after the reaction is completed, ethanol is removed by rotary evaporation to obtain an amination intermediate;

[0013] Furthermore, the dosage ratio of tetramethyltetravinylcyclotetrasiloxane, β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol is 0.1 mol: 0.4 mol: 50-80 mg: 120-160 mL. Under the promotion of dimethylphenylphosphine and initiation of ultraviolet radiation, β-mercaptoethylamine and tetramethyltetravinylcyclotetrasiloxane undergo click addition, and active amino groups are introduced to modify the structure of cyclotetrasiloxane.

[0014] Step A2: The aminated intermediate, ethyl methacrylate and anhydrous toluene are mixed, nitrogen is introduced for protection, the temperature is adjusted to 0-10° C. in an ice-water bath, and trimethylaluminum is slowly added with stirring. After the addition is complete, the temperature is raised to 40-55° C. and the reaction is continued for 6-8 hours. After the reaction is completed, the toluene is removed by vacuum rotary evaporation to obtain a modified monomer;

[0015] Furthermore, the usage ratio of the aminated intermediate, ethyl methacrylate, trimethylaluminum and anhydrous toluene is 0.1 mol: 0.4 mol: 20-30 mg: 80-100 mL. Under the promotion of trimethylaluminum, ethyl methacrylate and the amino group grafted by the aminated intermediate undergo amine ester exchange to form a multi-acrylate structure modification.

[0016] Step A3: premixing acrylic acid, butyl acrylate, hydroxypropyl acrylate, glycidyl methacrylate and a modified monomer as a composite substrate, adding an emulsifier and deionized water, mixing, heating to 80-90° C., intermittently adding an ammonium persulfate solution, controlling the total reaction time to be 3.2-3.8 h, cooling to room temperature after the reaction is completed, and adjusting the pH value to 9±0.2 with aqueous ammonia to obtain a water-based binder;

[0017] Furthermore, the molar ratio of acrylic acid, butyl acrylate, hydroxypropyl acrylate, glycidyl methacrylate and modified monomer is 1: 0.15-0.22: 0.4-0.5: 0.25-0.3: 0.18-0.26, the emulsifier is 5.5-7wt% of the composite substrate, the deionized water is 65-70wt% of the composite substrate, and the ammonium persulfate is 0.26-0.32wt% of the composite substrate.

[0018] Beneficial effects of the present invention:

[0019] The invention discloses a water-dispersible black ink, which does not add volatile harmful substances, is more environmentally friendly than solvent oil type ink, and has less damage to the health of construction workers; the ink uses an independently developed acrylic acid-based water-based connecting material as a film-forming material, and has good compatibility with common black pigments such as iron oxide black, manganese iron black and copper chrome black, and is prepared by click addition of β-mercaptoethylamine and tetramethyltetravinylcyclotetrasiloxane, introducing active amino groups to modify the ends of the cyclotetrasiloxane structure, and then ethyl methacrylate and its amino group are subjected to amine ester exchange, introducing multi-acrylate structure modification, and using the modified monomer as a modified monomer to copolymerize with acrylic acid, hydroxypropyl acrylate, etc. to form a water-based resin; the sulfur-nitrogen structure introduced into the macromolecular polymer chain by the modified monomer block forms a water-based resin. The modified monomer block introduces a cyclosiloxane structure into the macromolecular polymer chain, breaking the uniform chain structure. At the same time, it enriches the pigment by in-situ complexation, forming a multi-layer structure in the printing layer, which makes the printing layer have high color stiffness, moderate glossiness, and more comfortable for human eyes to observe. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1, preparing environmentally friendly black ink, as follows:

[0022] (1) Preparation of water-based binder

[0023] Step A1: β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol were mixed under nitrogen protection, and tetramethyltetravinylcyclotetrasiloxane was added and mixed, and the temperature was raised to 65°C and 180W / m 2 The mixture was irradiated with ultraviolet light, stirred at 80 rpm and refluxed for 3.5 h, wherein the dosage ratio of tetramethyltetravinylcyclotetrasiloxane, β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol was 0.1 mol: 0.4 mol: 50 mg: 120 mL. After the reaction, the ethanol was removed by rotary evaporation to obtain an amination intermediate.

[0024] Step A2: Take the aminated intermediate, ethyl methacrylate and anhydrous toluene, mix them, introduce nitrogen protection, adjust the temperature to 0°C in an ice-water bath, apply stirring at 180rpm, slowly add trimethylaluminum within 50min, raise the temperature to 40°C after complete addition, and continue to react for 8h, wherein the amount ratio of the aminated intermediate, ethyl methacrylate, trimethylaluminum and anhydrous toluene is 0.1mol:0.4mol:20mg:80mL. After the reaction is completed, remove toluene by reduced pressure rotary evaporation to obtain a modified monomer.

[0025] Step A3: Take acrylic acid, butyl acrylate, hydroxypropyl acrylate, glycidyl methacrylate and modified monomer, and premix them in a molar ratio of 1:0.15:0.5:0.25:0.26 to prepare a composite substrate. Then add 7wt% of the emulsifier NP-40 and 70wt% of the deionized water to the composite substrate, and heat to 80°C. Take the ammonium persulfate solution, divide it into three equal volumes, and add it intermittently for 15 minutes. After the addition is complete, continue to stir and react at a constant temperature. The total addition reaction time of ammonium persulfate is controlled to be 3.8 hours. After the reaction is completed, cool to room temperature, adjust the pH value to 9 with ammonia water, and allow the error to be 0.2 to obtain a water-based binder.

[0026] (2) Preparation of black ink

[0027] Ingredients: The raw materials are taken according to the weight percentage, 16wt% of metallic black pigment, in this implementation process, the iron oxide black ZL-330Q of Zhonglong Materials Group is used; 1.8wt% of covering agent, in the implementation process, the hydrophilic titanium dioxide NY-010A of Jiangsu Hehai Nano Technology Co., Ltd. is used; 0.25wt% of wetting agent, in the implementation process, TEGO-245 of Digo is used; 0.1wt% of leveling agent, in the implementation process, BYK-306 of BYK Chemical is used; 0.18wt% of defoaming agent, in the implementation process, BYK-022 of BYK Chemical is used; 1.6wt% of drying agent, in the implementation process, the water-based drying agent A-16 of Shanghai Tianyu Chemical Technology Co., Ltd. is used; 31wt% of distilled water; 49.07wt% of water-based connecting material is homemade in this embodiment.

[0028] Compounding: Premix the metallic black pigment, covering agent, wetting agent, leveling agent and distilled water at 360 rpm for 10 minutes, then add the aqueous binder and mix in a ball mill for 2 hours, filter out the grinding balls, add the drying agent to the ground material and mix well to obtain an environmentally friendly black ink.

[0029] Example 2, preparing environmentally friendly black ink, as follows:

[0030] (1) Preparation of water-based binder

[0031] Step A1: β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol were mixed under nitrogen protection, and tetramethyltetravinylcyclotetrasiloxane was added and mixed, and the temperature was raised to 75°C and assisted by 260W / m 2 The mixture was irradiated with ultraviolet light, stirred at 120 rpm and refluxed for 2.5 h, wherein the dosage ratio of tetramethyltetravinylcyclotetrasiloxane, β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol was 0.1 mol: 0.4 mol: 80 mg: 160 mL. After the reaction, the ethanol was removed by rotary evaporation to obtain an amination intermediate.

[0032] Step A2: Take the aminated intermediate, ethyl methacrylate and anhydrous toluene, mix them, introduce nitrogen protection, adjust the temperature to 10°C in an ice-water bath, apply stirring at 240rpm, slowly add trimethylaluminum within 30min, raise the temperature to 55°C after complete addition, and continue to react for 6h, wherein the amount ratio of the aminated intermediate, ethyl methacrylate, trimethylaluminum and anhydrous toluene is 0.1mol:0.4mol:30mg:100mL. After the reaction is completed, remove toluene by reduced pressure rotary evaporation to obtain a modified monomer.

[0033] Step A3: Take acrylic acid, butyl acrylate, hydroxypropyl acrylate, glycidyl methacrylate and modified monomer, and premix them in a molar ratio of 1:0.22:0.4:0.3:0.18 as a composite substrate, then add 5.5wt% of emulsifier NP-40 and 65wt% of deionized water to the composite substrate, mix, heat to 90°C, take ammonium persulfate solution, divide it into three equal volumes, add it intermittently for 15 minutes, continue to stir and react at a constant temperature after complete addition, control the total addition reaction time of ammonium persulfate to be 3.2 hours, cool to room temperature after the reaction is completed, adjust the pH value to 9 with ammonia water, and allow the error to be 0.2 to obtain a water-based binder.

[0034] (2) Preparation of black ink

[0035] Ingredients: The raw materials are taken according to the weight percentage, 21wt% of metallic black pigment, in this implementation process, the manganese iron black Black-3050 of Zhonglong Materials Group is used; 2.2wt% of covering agent, in the implementation process, the hydrophilic titanium dioxide NY-010A of Jiangsu Hehai Nano Technology Co., Ltd. is used; 0.3wt% of wetting agent, in the implementation process, TEGO-245 of Digo is used; 0.15wt% of leveling agent, in the implementation process, BYK-306 of BYK Chemical is used; 0.12wt% of defoaming agent, in the implementation process, BYK-022 of BYK Chemical is used; 1.3wt% of drying agent, in the implementation process, the water-based drying agent A-16 of Shanghai Tianyu Chemical Technology Co., Ltd. is used; 26wt% of distilled water; 48.93wt% of water-based connecting material is homemade in this embodiment.

[0036] Compounding: Premix the metallic black pigment, covering agent, wetting agent, leveling agent and distilled water at 360 rpm for 10 minutes, then add the aqueous binder and mix in a ball mill for 2 hours, filter out the grinding balls, add the drying agent to the ground material and mix well to obtain an environmentally friendly black ink.

[0037] Example 3, preparing environmentally friendly black ink, as follows:

[0038] (1) Preparation of water-based binder

[0039] Step A1: β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol were mixed under nitrogen protection, and tetramethyltetravinylcyclotetrasiloxane was added and mixed, and the temperature was raised to 70°C and assisted by 220W / m 2 The mixture was irradiated with ultraviolet light, stirred at 120 rpm and refluxed for 3.2 h, wherein the dosage ratio of tetramethyltetravinylcyclotetrasiloxane, β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol was 0.1 mol: 0.4 mol: 70 mg: 150 mL. After the reaction, the ethanol was removed by rotary evaporation to obtain an amination intermediate.

[0040] Step A2: Take the aminated intermediate, ethyl methacrylate and anhydrous toluene, mix them, introduce nitrogen protection, adjust the temperature to 5°C in an ice-water bath, apply stirring at 240rpm, slowly add trimethylaluminum within 50min, raise the temperature to 45°C after complete addition, and continue to react for 7h, wherein the amount ratio of the aminated intermediate, ethyl methacrylate, trimethylaluminum and anhydrous toluene is 0.1mol:0.4mol:30mg:90mL. After the reaction is completed, remove toluene by reduced pressure rotary evaporation to obtain a modified monomer.

[0041] Step A3: Take acrylic acid, butyl acrylate, hydroxypropyl acrylate, glycidyl methacrylate and modified monomer, and premix them in a molar ratio of 1:0.18:0.45:0.27:0.24 as a composite substrate, then add 6.2wt% of emulsifier NP-40 and 68wt% of deionized water to the composite substrate, mix, heat to 85°C, take ammonium persulfate solution, divide it into three equal volumes, add it intermittently for 15 minutes, continue to stir and react at a constant temperature after complete addition, control the total addition reaction time of ammonium persulfate to be 3.5 hours, cool to room temperature after the reaction is completed, adjust the pH value to 9 with ammonia water, and allow the error to be 0.2 to obtain an aqueous binder.

[0042] (2) Preparation of black ink

[0043] Ingredients: The raw materials are taken according to the weight percentage, 19wt% of metallic black pigment, and the copper chromium black Black-2300K of Zhonglong Materials Group is used in this implementation process; 2.1wt% of covering agent, and the hydrophilic titanium dioxide NY-010A of Jiangsu Hehai Nano Technology Co., Ltd. is used in the implementation process; 0.28wt% of wetting agent, and TEGO-245 of Digo is used in the implementation process; 0.12wt% of leveling agent, and BYK-306 of BYK Chemical is used in the implementation process; 0.15wt% of defoaming agent, and BYK-022 of BYK Chemical is used in the implementation process; 1.4wt% of drying agent, and the water-based drying agent A-16 of Shanghai Tianyu Chemical Technology Co., Ltd. is used in the implementation process; 28wt% of distilled water; 48.95wt% of water-based connecting material is homemade in this embodiment.

[0044] Compounding: Premix the metallic black pigment, covering agent, wetting agent, leveling agent and distilled water at 360 rpm for 10 minutes, then add the aqueous binder and mix in a ball mill for 2 hours, filter out the grinding balls, add the drying agent to the ground material and mix well to obtain an environmentally friendly black ink.

[0045] In a comparative example, a commercially available water-based acrylic emulsion binder was used to prepare a black ink, as follows:

[0046] Ingredients: The raw materials are taken according to the weight percentage, 20wt% of metallic black pigment, the iron oxide black ZL-330Q of Zhonglong Materials Group is used in this implementation process; 2wt% of covering agent, the hydrophilic titanium dioxide NY-010A of Jiangsu Hehai Nano Technology Co., Ltd. is used in the implementation process; 0.28wt% of wetting agent, TEGO-245 of Digo is used in the implementation process; 0.12wt% of leveling agent, BYK-306 of BYK Chemical is used in the implementation process; 0.15wt% of defoaming agent, BYK-022 of BYK Chemical is used in the implementation process; 1.4wt% of drying agent, the water-based drying agent A-16 of Shanghai Tianyu Chemical Technology Co., Ltd. is used in the implementation process; 27wt% of distilled water; 49.05wt% of water-based acrylic emulsion connecting material, WPA4413 product of Guangzhou Huigu Chemical Co., Ltd.

[0047] Compounding: Premix the metallic black pigment, covering agent, wetting agent, leveling agent and distilled water at 360 rpm for 10 minutes, then add the aqueous binder and mix in a ball mill for 2 hours, filter out the grinding balls, add the drying agent to the ground material and mix well to obtain an environmentally friendly black ink.

[0048] The ink prepared as above was sampled for stability test, including: storage stability test, the sample ink was placed in a universal stability analyzer, the test temperature was 60±2°C, the sample storage height was 20mm, and the test period was 24h; sedimentation stability test, using the specific absorbance method, specifically, the above sample was diluted 1000 times with deionized water, the initial absorbance was measured by ultraviolet spectrophotometer, and then the diluted sample was placed in a centrifuge, centrifuged at 1800rpm for 30min, and the centrifugal absorbance was measured again, then the specific absorbance = centrifugal absorbance / initial absorbance × 100%; the specific test data are shown in Table 1:

[0049] Table 1

[0050] Example 1 Example 2 Example 3 Comparative Example TSI Index 0.16 0.22 0.18 0.47 Specific absorbance / % 91.2 87.9 90.5 53.2

[0051] From the test results in Table 1, it can be seen that the ink prepared in the embodiment has a TSI index of only 0.16-0.22 and a specific absorbance of 87.9-91.2%. Compared with the comparative example, the ink has excellent stability, is easy to construct and has a positive significance for improving the printing quality.

[0052] The ink prepared as above was sampled and printed on PET as the substrate. After drying for 24 hours, a printed sample was prepared. The glossiness of the printed layer was tested according to GB / T 9754-2007, the adhesion fastness of the printed layer was tested according to GB / T 13217.7-2009, and the tolerance of the printed layer was tested according to GB / T 18724-2008. The specific test results are shown in Table 2:

[0053] Table 2

[0054] Example 1 Example 2 Example 3 Comparative Example Glossiness (60°) / % 79.1 72.5 74.9 90.7 Adhesion fastness / % 100 100 100 93 Alkali resistance (1% NaOH) No shedding or discoloration No shedding or discoloration No shedding or discoloration No shedding or discoloration Alkali resistance (1% HCl) No shedding or discoloration No shedding or discoloration No shedding or discoloration No shedding or discoloration

[0055] It can be seen from the test results in Table 2 that the inks of the embodiments and comparative examples are bright black inks with good tolerance. Among them, the 60° glossiness of the ink printing layer of the embodiments reaches 72.5-79.1%, which is moderate in glossiness compared to the comparative example, between semi-matte and high gloss, and is more comfortable for human eyes to observe. There is no visible falling off in the adhesion fastness test, the adhesion fastness reaches 100%, and the printing layer has good stability.

[0056] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0057] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A process for preparing an environmentally friendly black ink, characterized in that: The specific operation is: premix the metallic black pigment, covering agent, wetting agent, leveling agent and distilled water, then add the water-based binder, grind and disperse, filter, and then add the drying agent to mix well to obtain the environmentally friendly black ink; The aqueous vehicle is prepared by the following method: Step A1: Dissolve β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol under nitrogen protection, add tetramethyltetravinylcyclotetrasiloxane and mix well, heat to 65-75°C, and heat with 180-260W / m 2 UV irradiation, stirring and reflux for 2.5-3.5h, after the reaction is completed, ethanol is removed by rotary evaporation to obtain an amination intermediate; Step A2: The aminated intermediate, ethyl methacrylate and anhydrous toluene are mixed, nitrogen is introduced for protection, the temperature is adjusted to 0-10° C. in an ice-water bath, and trimethylaluminum is slowly added with stirring. After the addition is complete, the temperature is raised to 40-55° C. and the reaction is continued for 6-8 hours. After the reaction is completed, the toluene is removed by vacuum rotary evaporation to obtain a modified monomer; Step A3: premix acrylic acid, butyl acrylate, hydroxypropyl acrylate, glycidyl methacrylate and modified monomer as a composite substrate, add an emulsifier and deionized water to mix, heat to 80-90° C., intermittently add ammonium persulfate solution, control the total addition reaction time of ammonium persulfate to be 3.2-3.8 h, cool to room temperature after the reaction is completed, adjust the pH value to 9±0.2 with ammonia water, and obtain a water-based binder.

2. The process for preparing an environmentally friendly black ink according to claim 1, characterized in that: The usage ratio of tetramethyltetravinylcyclotetrasiloxane, β-mercaptoethylamine, dimethylphenylphosphine and anhydrous ethanol is 0.1 mol: 0.4 mol: 50-80 mg: 120-160 mL.

3. The process for preparing an environmentally friendly black ink according to claim 2, characterized in that: The usage ratio of the amination intermediate, ethyl methacrylate, trimethylaluminum and anhydrous toluene is 0.1 mol: 0.4 mol: 20-30 mg: 80-100 mL.

4. The process for preparing an environmentally friendly black ink according to claim 3, characterized in that: The molar ratio of acrylic acid, butyl acrylate, hydroxypropyl acrylate, glycidyl methacrylate and modified monomer is 1: 0.15-0.22: 0.4-0.5: 0.25-0.3: 0.18-0.26, the emulsifier is 5.5-7wt% of the composite substrate, the deionized water is 65-70wt% of the composite substrate, and the ammonium persulfate is 0.26-0.32wt% of the composite substrate.

5. The process for preparing an environmentally friendly black ink according to claim 1, characterized in that: The proportions of raw materials in the environmentally friendly black ink are: metallic black pigment 16-21wt%, opacifier 1.8-2.2wt%, wetting agent 0.25-0.3wt%, leveling agent 0.1-0.15wt%, defoaming agent 0.12-0.18wt%, drying agent 1.3-1.6wt% and distilled water 26-31wt%, and the rest is water-based binder.

6. The process for preparing an environmentally friendly black ink according to claim 5, characterized in that: The metallic black pigment is one of iron oxide black, manganese iron black and copper chrome black.

7. The process for preparing an environmentally friendly black ink according to claim 5, characterized in that: The covering agent is hydrophilic titanium dioxide.

Citation Information

Patent Citations

  • Preparation method for POSS / PDMAEMA organic / inorganic hybrid material according to thiol-ene click chemistry method

    CN104558321A

  • Preparation method of ultraviolet-curable transparent acrylate polysiloxane coating

    CN108913023A