Dynamic mechanical properties testing device and testing method for cover glass

By designing a dynamic mechanical performance testing device for cover glass, including an impact rod, an incident rod, a clamping device and a transmission rod, and using a waveform shaper and a transmission rod to collect signals, it solves the difficulty in testing the dynamic bending of brittle materials in the existing technology. To solve the problem of strength, high-precision dynamic bending mechanical properties testing of cover glass for electronic equipment is achieved.

CN118641329BActive Publication Date: 2024-10-18BEIJING UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411109929.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-18
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

It is difficult to effectively test the dynamic mechanical properties of brittle materials with existing technology. Especially under the structure of sheet glass cover, it is difficult to accurately obtain the dynamic bending strength, which makes it difficult to solve the problem of glass failure when the mobile phone is dropped.

Method used

A dynamic mechanical performance testing device including an impact rod, an incident rod, a clamping device and a transmission rod is designed. The rising edge of the incident pulse is delayed through a waveform shaper, the clamping device provides line contact support, and the transmission rod collects the transmitted wave signal and conducts Load balance verification enables testing of the dynamic bending mechanical properties of cover glass.

Benefits of technology

It improves the accuracy of experimental data, can directly measure dynamic bending strength, satisfies the one-dimensional stress wave propagation conditions, provides effective research on the dynamic bending mechanical properties of electronic equipment cover glass, and solves the problem of low accuracy in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118641329B_ABST
    Figure CN118641329B_ABST
Patent Text Reader

Abstract

The invention relates to a dynamic mechanical property testing device and a testing method for cover glass. The testing device comprises an impact rod, an incident rod, a clamping device and a transmission rod. The incident rod, the impact rod and the transmission rod are all cylindrical slender rods and are all arranged horizontally. A waveform shaper is provided on the circular end surface of the incident rod facing the impact rod, which is used to delay the rising edge of the incident pulse. One end of the incident rod facing the clamping device is wedge-shaped, and the head of the wedge is provided with an arc-shaped end surface protruding toward the clamping device, which is used to contact and apply force to the cover glass on the clamping device. The clamping device is arranged vertically, and two supporting parts are provided on the front side, which protrude toward the incident rod and form line contact with the cover glass. The back side of the clamping device is connected to one end of the transmission rod, and the transmission rod is hollow.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of dynamic mechanical property testing of cover glass, and in particular relates to a dynamic mechanical property testing device and a testing method for cover glass. Background Art

[0002] With the continuous development of electronic technology, the types and functions of various smart electronic devices are becoming more and more abundant, such as smartphones, e-readers, tablets, etc. Silicate glass has a series of excellent chemical and physical properties such as high transparency, good stability, high hardness, and strong compressive resistance, and is widely used in the display cover structure of handheld electronic devices. Taking smartphones as an example, due to considerations of appearance design and visual experience, the screen-to-body ratio of smartphones is getting higher and higher. Some manufacturers have also launched flagship models with curved screens, and the battery cover on the back of some models is also made of glass, making the problem of cover glass failure caused by the impact of the phone falling a major pain point and structural design difficulty in the industry.

[0003] It is generally believed that brittle materials have a certain strain rate effect, and the material strength under dynamic loading conditions is higher than the quasi-static strength. When a mobile phone falls, the main cause of glass failure is tensile fracture caused by bending deformation. Accurately obtaining the dynamic mechanical properties of electronic device cover glass can provide important data support for its drop reliability assessment. Existing dynamic mechanical properties test methods for brittle materials are mostly concentrated on uniaxial compression and Brazilian disk splitting loading forms, which are difficult to apply to sheet glass cover structures. Summary of the invention

[0004] In view of the above problems, the present invention provides a dynamic mechanical property testing device and a testing method for cover glass, wherein the testing device comprises an impact rod, an incident rod, a clamping device and a transmission rod, wherein the incident rod, the impact rod and the transmission rod are all cylindrical slender rods and are all arranged horizontally; a waveform shaper is provided on the circular end surface of the incident rod facing the impact rod, which is used to delay the rising edge of the incident pulse; one end of the incident rod facing the clamping device is wedge-shaped, and the head of the wedge is provided with an arc-shaped end surface protruding toward the clamping device, which is used to contact and apply force to the cover glass on the clamping device;

[0005] The clamping device is arranged vertically, and two supporting parts are arranged on the front side, which protrude toward the incident rod and form a line contact with the cover glass; the back side of the clamping device is connected to one end of the transmission rod, and the transmission rod is hollow.

[0006] Optionally, the impact rod is a solid cylinder, and both ends of the impact rod are smooth and flat circular end faces. The impact rod can withstand the compressed air acceleration of the air cannon, so that the head end face of the impact rod hits the waveform shaper at the tail of the incident rod.

[0007] Optionally, the waveform shaper is in the shape of a circular sheet, and its diameter is not greater than the diameter of the end face of the incident rod, and the waveform shaper is concentrically arranged with the incident rod; the material of the waveform shaper is red copper.

[0008] Optionally, the incident rod is a solid cylinder with a horizontal central axis; the tail of the incident rod is a smooth and flat circular end surface, the head is wedge-shaped, a striking part is provided at the center of the wedge-shaped head, the tail of the striking part is connected to the incident rod and is integrally formed, and the head of the striking part protrudes outward and is a section of an arc surface;

[0009] The central axis of the arc surface is horizontal and perpendicular to the central axis of the incident rod, the central axis of the arc surface passes through the central axis of the incident rod, and the length of the central axis of the arc surface is equal to the diameter of the end face of the incident rod.

[0010] Further optionally, the arc of the arc surface of the impact portion is 2.09-3.84 rad.

[0011] Optionally, the cover glass is a rectangular thin sheet sample.

[0012] Optionally, the front of the clamping device is vertical, and includes a bottom surface, a supporting surface, a supporting portion and an outer edge surface from the inside to the outside, the bottom surface, the supporting surface and the outer edge surface are all smooth and flat planes, the bottom surface is in the middle of the clamping device, and a supporting surface is provided on the upper and lower sides of the bottom surface respectively, the angle between the supporting surface and the bottom surface is an obtuse angle, one side of the supporting portion is connected to the supporting surface, and the other side is connected to the outer edge surface, and the other side of the outer edge surface is connected to the top surface or the bottom surface of the clamping device. The upper and lower supporting portions provide double-point support for the cover glass.

[0013] Further optionally, the tail of the support part is adjacent to the main body of the clamping device, the head protrudes toward the direction of the incident rod, and is a section of an arc surface, the central axis of the arc surface of the support part is parallel to the central axis of the arc surface of the impact part, and the length of the central axis of the arc surface of the support part is equal to the width of the clamping device.

[0014] Further optionally, the arc surface of the support portion has an radian of 2.09-3.84 rad.

[0015] Further optionally, four hollow bars are provided on the wall surface of the transmission rod, and the four hollow bars are evenly arranged along the circumference of the transmission rod. The length of the hollow bars is slightly smaller than the length of the transmission rod, so that the two ends of the hollow bars do not extend to the two ends of the transmission rod.

[0016] Optionally, the impact rod, incident rod, clamping device and transmission rod are made of the same material, all of which are high-strength aluminum alloy; the impact rod, incident rod and transmission rod have the same outer diameter, and the central axes of the three are on the same horizontal line, and the centers of the cover glass and the clamping device are also on this horizontal line.

[0017] The present invention also provides a testing method for directly measuring the dynamic bending strength of cover glass, comprising the following steps:

[0018] (1) Arrange the force-applying device, the impact rod, the waveform shaper, the incident rod, the clamping device, and the transmission rod horizontally along the same axis in sequence; adhere strain gauges to the middle of the outer side surface of the incident rod and the middle of the outer side surface of the transmission rod respectively, and connect the strain gauges to the data analysis device;

[0019] (2) The cover glass is placed between the incident rod and the clamping device. The incident rod and the clamping device apply a pre-tightening force to the cover glass so that the cover glass does not fall off;

[0020] (3) The high-pressure gas of the force-applying device drives the impact rod, so that the impact rod hits the waveform shaper of the incident rod, generating a compression stress wave, which propagates in the incident rod to the cover glass and performs impact loading on the cover glass, generating a reflection wave that is reflected back to the incident rod, and at the same time generating a transmission wave that propagates along the transmission rod;

[0021] (4) The voltage data is collected and recorded by the strain gauges of the incident rod and the transmitted rod to obtain the original waveform. The dynamic bending load curve and loading speed time curve of the incident rod and the transmitted rod are then analyzed and obtained to obtain the dynamic bending strength.

[0022] Compared with the prior art, the present invention can use a hollow transmission rod to collect transmission wave signals and perform load balance verification. The clamping device can effectively support the cover glass and meet the one-dimensional stress wave propagation conditions. The transmission rod uses a thin-walled circular tube to amplify the signal, which greatly improves the accuracy of the experimental data. The test method solves the problem of dynamic mechanical property testing of brittle materials and can perform dynamic bending mechanical property experimental research on electronic equipment cover glass.

[0023] Optionally, in step (1), the transmission rod is supported by two brackets, the clamping device is also supported along with the transmission rod, the incident rod is supported by two brackets, the waveform shaper is also supported along with the incident rod, the impact rod is supported by two brackets, and the force-applying device is an air cannon.

[0024] Optionally, in step (2), the incident rod is tied to the bracket of the incident rod close to the cover glass with a rubber band to provide a force in the direction of the cover glass for the incident rod; the transmission rod is tied to the bracket of the transmission rod close to the cover glass with a rubber band to provide a force in the direction of the cover glass for the transmission rod, so that the incident rod and the transmission rod can apply forces in opposite directions to the cover glass, thereby clamping the cover glass.

[0025] The impact part of the incident rod is in line contact with the cover glass, and the two supporting parts of the clamping device are also in line contact with the cover glass, so that three-point bending loading of the cover glass is achieved.

[0026] Optionally, in step (4), the voltage data is the voltage signal measured by two strain gauges, and then the original waveform is obtained, in which the ordinate is the voltage signal, the unit is V; the abscissa is the time, the unit is μs; through the bridge theory, the voltage signal can be converted into the strain time history data of the incident wave , strain time history data of reflected wave Strain time history data of the transmitted wave ;

[0027] Then calculate the bending load F(t) and bending stress of the transmission rod and the incident rod and loading speed v(t), and obtain the dynamic bending stress curve and the loading speed time history curve. The ordinate of the dynamic bending stress curve is the bending stress, with the unit of MPa, and the ordinate of the loading speed time history curve is the loading speed, with the unit of m / s. The abscissas of the two curves are both time t, with the unit of μs. The bending stress at different times can be obtained according to the dynamic bending stress curve, and the highest point of the dynamic bending stress curve is the bending strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a structural schematic diagram of a dynamic mechanical properties testing device for cover glass;

[0029] Figure 2 A schematic diagram of a support portion and an impact portion clamping a cover glass;

[0030] Figure 3 is a schematic diagram of a transmission rod;

[0031] Figure 4 This is the original waveform obtained from the test;

[0032] Figure 5 The dynamic bending stress curve and loading speed time history curve obtained from the test.

[0033] In the accompanying drawings, 1-impact rod, 2-incident rod, 3-clamping device, 4-transmission rod, 5-waveform shaper, 6-cover glass, 7-support part, 8-impact part, 9-bottom surface, 10-support surface, 11-outer edge surface, 12-hollow strip. DETAILED DESCRIPTION

[0034] This embodiment provides a dynamic mechanical properties testing device for cover glass, such as Figure 1-Figure 3As shown, it includes an impact rod 1, an incident rod 2, a clamping device 3 and a transmission rod 4, the incident rod 2, the impact rod 1 and the transmission rod 4 are all cylindrical slender rods, and are all arranged horizontally; a waveform shaper 5 is provided on the circular end surface of the incident rod 2 facing the impact rod 1, which is used to delay the rising edge of the incident pulse; the end of the incident rod 2 facing the clamping device 3 is wedge-shaped, and the head of the wedge is provided with an arc-shaped end surface protruding toward the clamping device 3, which is used to contact and apply force to the cover glass 6 on the clamping device 3;

[0035] The clamping device 3 is vertically arranged, and two supporting parts 7 are provided on the front side, which protrude toward the incident rod 2 and form a line contact with the cover glass 6; the back side of the clamping device 3 is connected to one end of the transmission rod 4, and the transmission rod 4 is hollow.

[0036] The impact rod 1 is a solid cylinder, and both ends of the impact rod 1 are smooth and flat circular end faces. The impact rod 1 can withstand the compressed air acceleration of the air cannon, so that the head end face of the impact rod 1 hits the waveform shaper 5 at the tail of the incident rod 2.

[0037] The waveform shaper 5 is a circular sheet, and its diameter is not greater than the diameter of the end face of the incident rod 2. The waveform shaper 5 is concentric with the incident rod 2. The waveform shaper 5 is made of copper and has a thickness of 2 mm. The waveform shaper 5 can effectively extend the time of the rising edge of the incident wave and the incident wavelength, improve the test accuracy, and promote the realization of the constant rate loading process.

[0038] The incident rod 2 is a solid cylinder with a horizontal central axis; the tail of the incident rod 2 is a smooth and flat circular end surface, the head is wedge-shaped, and a striking portion 8 is provided at the center of the wedge-shaped head. The tail of the striking portion 8 is connected to the incident rod 2 and is integrally formed, and the head of the striking portion 8 protrudes outward and is a section of an arc surface;

[0039] The central axis of the arc surface of the impact part 8 is horizontal and perpendicular to the central axis of the incident rod 2, and the central axis of the arc surface of the impact part 8 passes through the central axis of the incident rod 2. The length of the central axis of the arc surface of the impact part 8 is equal to the diameter of the end face of the incident rod 2. When the impact part 8 impacts the cover glass 6, it forms a line contact with the cover glass 6.

[0040] The arc of the arc surface of the impact portion 8 is 3.14 rad, and the corresponding angle is 180°, that is, a semicircular surface.

[0041] The cover glass 6 is a rectangular thin sheet sample.

[0042] The front of the clamping device 3 is vertical, and includes a bottom surface 9, a support surface 10, a support portion 7 and an outer edge surface 11 from the inside to the outside. The bottom surface 9, the support surface 10 and the outer edge surface 11 are all smooth and flat planes. The bottom surface 9 is located in the middle of the clamping device 3. A support surface 10 is provided on the upper and lower sides of the bottom surface 9 respectively. The angle between the support surface 10 and the bottom surface 9 is an obtuse angle. One side of the support portion 7 is connected to the support surface 10, and the other side is connected to the outer edge surface 11. The other side of the outer edge surface 11 is connected to the top surface or the bottom surface of the clamping device 3. The upper and lower support portions 7 support the cover glass 6 at two points.

[0043] When the clamping device 3 clamps the cover glass 6 , the distances between the support portion 7 , the outer edge surface 11 , the bottom surface 9 and the cover glass 6 gradually increase.

[0044] The tail of the support part 7 is adjacent to the main body of the clamping device 3, and the head protrudes toward the incident rod 2 and is a section of an arc surface. The central axis of the arc surface of the support part 7 is parallel to the central axis of the arc surface of the impact part 8, and the length of the central axis of the arc surface of the support part 7 is equal to the width of the clamping device 3.

[0045] The arc of the arc surface of the support portion 7 is 3.14 rad, and the corresponding angle is 180°, that is, a semicircular surface. The two lines of the two support portions 7 supporting the cover glass 6 are parallel to each other and are 12 mm apart from each other.

[0046] The back of the clamping device 3 is vertical and fixedly connected to the head of the transmission rod 4. The transmission rod 4 is a round tube, and the back of the clamping device 3 can fully cover the end face of the head of the transmission rod 4. The back of the clamping device 3 can be connected to the transmission rod 4 using high-strength glue.

[0047] Four hollow strips 12 are provided on the wall surface of the transmission rod 4, so that the internal space of the transmission rod 4 is connected to the external space, reducing the cross-sectional area of ​​the transmission rod 4, so as to amplify the test signal and improve the accuracy of the test;

[0048] The four hollow strips 12 are evenly arranged along the circumference of the transmission rod 4 . The length of the hollow strips 12 is slightly smaller than the length of the transmission rod 4 , so that the two ends of the hollow strips 12 do not extend to the two ends of the transmission rod 4 .

[0049] The area of ​​one hollow strip 12 accounts for 5-8% of the side area of ​​the transmission rod.

[0050] Due to the low bending fracture strength of brittle materials, the transmission signal generated by conventional transmission rods is small, low in precision, and difficult to collect. The present invention uses hollow and hollow transmission rods to effectively amplify the transmission signal and improve the precision of experimental test data. The present invention unexpectedly found that the hollow form has a better effect of amplifying the transmission signal than other groove-type designs and is easy to process.

[0051] The impact rod 1, the incident rod 2, the clamping device 3 and the transmission rod 4 are made of the same material, which is high-strength aluminum alloy; the impact rod 1, the incident rod 2 and the transmission rod 4 have the same outer diameter, and the central axes of the three are on the same horizontal line, and the centers of the cover glass 6 and the clamping device 3 are also on this horizontal line.

[0052] This embodiment provides a testing method for directly measuring the dynamic bending strength of the cover glass 6, using the above-mentioned testing device, including the following steps:

[0053] (1) The force applying device, the impact rod 1, the waveform shaper 5, the incident rod 2, the clamping device 3, and the transmission rod 4 are horizontally arranged in sequence along the same axis; strain gauges are respectively attached to the middle of the outer side surface of the incident rod 2 and the middle of the outer side surface of the transmission rod 4, and the strain gauges are connected to the data analysis device;

[0054] (2) The cover glass 6 is placed between the incident rod 2 and the clamping device 3. The incident rod 2 and the clamping device 3 apply a pre-tightening force to the cover glass 6 so that the cover glass 6 does not fall off;

[0055] (3) The high-pressure gas of the force-applying device drives the impact rod 1, so that the impact rod 1 impacts the waveform shaper 5 of the incident rod 2, generating a compression stress wave, which propagates in the incident rod 2 to the cover glass 6 and performs impact loading on the cover glass 6, generating a reflection wave that is reflected back to the incident rod, and generating a transmission wave that propagates along the transmission rod 4;

[0056] (4) The voltage data is collected and recorded by the strain gauges of the incident rod and the transmitted rod to obtain the original waveform. The dynamic bending load curve and loading speed time curve of the incident rod and the transmitted rod are then analyzed and obtained to obtain the dynamic bending strength.

[0057] In step (1), the transmission rod 4 is supported by two brackets, the clamping device 3 is also supported along with the transmission rod 4, the incident rod 2 is supported by two brackets, the waveform shaper 5 is also supported along with the incident rod 2, the impact rod 1 is supported by two brackets, and the force-applying device is an air cannon.

[0058] In step (2), the incident rod 2 is tied to the bracket of the incident rod 2 close to the cover glass 6 by a rubber band to provide a force for the incident rod 2 in the direction of the cover glass 6; the transmission rod 4 is tied to the bracket of the transmission rod 4 close to the cover glass 6 by a rubber band to provide a force for the transmission rod 4 in the direction of the cover glass 6, so that the incident rod 2 and the transmission rod 4 can apply forces in opposite directions to the cover glass 6, thereby clamping the cover glass 6.

[0059] The impact portion 8 of the incident rod 2 is in line contact with the cover glass 6 , and the two support portions 7 of the clamping device 3 are also in line contact with the cover glass 6 , thereby achieving three-point bending loading on the cover glass 6 .

[0060] In step (3), the impact rod 1 impacts the waveform shaper 5 along the axial direction at a certain speed and generates a compressive stress wave. The stress wave propagates in the incident rod 2 to the cover glass 6. The cover glass 6 is supported by the clamping device 3, generating a reflected wave and propagating in the reverse direction along the incident rod 2. At the same time, a transmitted wave is generated and propagated along the transmission rod 4.

[0061] In step (4), the voltage data is the voltage signal measured by the two strain gauges, and then the original waveform is obtained. The ordinate in the figure is the voltage signal, the unit is V; the abscissa is the time, the unit is μs; through the bridge theory, the voltage signal can be converted into the strain time history data of the incident wave , strain time history data of reflected wave Strain time history data of the transmitted wave ;

[0062] Then calculate the bending load F(t) and bending stress of the transmission rod and the incident rod and loading speed v(t), and obtain the dynamic bending stress curve and the loading speed time history curve. The ordinate of the dynamic bending stress curve is the bending stress, with the unit of MPa, and the ordinate of the loading speed time history curve is the loading speed, with the unit of m / s. The abscissas of the two curves are both time t, with the unit of μs. The bending stress at different times can be obtained according to the dynamic bending stress curve, and the highest point of the dynamic bending stress curve is the bending strength.

[0063] The bending load obtained from the incident and reflected waves is given by the following formula:

[0064] ;

[0065] Where, t is time, μs; E I is the elastic modulus of the incident rod, MPa; A I is the cross-sectional area of ​​the incident rod, 78.5 mm 2 ;

[0066] The bending load obtained from the transmitted wave is determined by the following formula:

[0067] ;

[0068] Among them, E T is the elastic modulus of the transmission rod, MPa; A T is the cross-sectional area of ​​the transmission rod, 22.6 mm 2 ;

[0069] The elastic modulus is related to the material of the rod. The incident rod and the transmission rod are made of the same material, and their elastic moduli are also the same, specifically 72000MPa. The units of the above bending loads are all N.

[0070] The bending stress resulting from the incident and reflected waves is determined by the following formula:

[0071] ;

[0072] The bending stress obtained from the transmitted wave is determined by the following formula:

[0073] ;

[0074] Wherein, L is the span of the cover glass, that is, the distance between two lines of the cover glass supported by two supporting parts, 12 mm; b is the width of the cover glass, 4 mm; h is the height of the cover glass, 2 mm; the units of the above bending stresses are all MPa.

[0075] Due to the loading displacement ,

[0076] Loading speed ,

[0077] Wherein, C0 is the stress wave velocity in the incident rod or the transmitted rod. Since the incident rod and the transmitted rod are made of the same material, C0 is specifically 5000 m / s; the unit of loading speed is m / s.

[0078] After obtaining the original test data (i.e., the voltage signals measured by the two strain gauges), the dynamic bending stress curve and loading speed time history curve of the cover glass can be calculated by the above formula. The amount of original test data is relatively large, and the above curves are composed of a large number of data points, which are processed by Microsoft Excel or other professional data processing programs.

[0079] The typical original waveform formed by the original test data is as follows: Figure 4 As shown in the figure, it can be seen that through the shaping effect of the waveform shaper, the rising edge of the incident wave slows down and presents a trapezoidal wave form; the transmitted wave is a triangular wave, and the amplitude of the transmitted wave is effectively amplified due to the use of hollow and hollow transmission rods; the initial stage of the reflected wave presents a step-like shape, and its platform segment shows that the loading condition of the sample is basically reached during the loading process. The descending segment of the first peak of the transmitted wave corresponds to the descending segment after the platform segment of the reflected wave, which represents the fracture damage of the sample.

[0080] After data processing, the dynamic bending stress curve is obtained as follows: Figure 5 As shown, the curve marked with a triangle represents the dynamic bending stress curve (first curve) obtained using the incident wave and reflected wave data, and the curve marked with a circle represents the dynamic bending stress curve (second curve) obtained using the transmitted wave data; the two curves basically overlap, indicating that during the loading process, the load between the incident rod and the cover glass, and the load between the transmitted rod and the cover glass are basically balanced.

[0081] Figure 5 The dotted line in the figure is the loading speed time history curve. It can be seen that in the main loading stage (15-50μs), the loading speed is stable at about 1m / s, which proves that this experiment can ensure constant rate loading.

[0082] The present invention defines the dynamic bending load balance factor , which is expressed as follows:

[0083] ;

[0084] in, and They are Figure 5 The bending stress values ​​corresponding to the first curve and the second curve at the same time.

[0085] If during the loading process, the starting point is when the bending stress value of any dynamic bending stress curve reaches 40% of the bending stress peak value of the corresponding curve, and the end point is the peak value of any dynamic bending stress curve. If the value is always less than 10%, it is considered that the loads between the incident rod, the transmission rod and the sample are in a balanced state during the loading process.

[0086] In the initial stage of dynamic loading, the cover glass bears a lower load, that is, the initial bending stress value is small. The detection accuracy of existing detection equipment is limited, which is easy to cause large errors. In addition, this stage has little impact on the mechanical test of the cover glass. Therefore, this stage is not included in the consideration of the above-mentioned balance factor.

Claims

1. A dynamic mechanical properties testing device for cover glass, characterized in that: It includes an impact rod, an incident rod, a clamping device and a transmission rod. The incident rod, the impact rod and the transmission rod are all cylindrical slender rods and are all arranged horizontally. A waveform shaper is provided on the circular end surface of the incident rod facing the impact rod, which is used to delay the rising edge of the incident pulse. One end of the incident rod facing the clamping device is wedge-shaped, and the head of the wedge is provided with an arc-shaped end surface protruding toward the clamping device, which is used to contact and apply force to the cover glass on the clamping device. The clamping device is arranged vertically, and two supporting parts are arranged on the front side, and the supporting parts protrude toward the incident rod and form a line contact with the cover glass; The back side of the clamping device is connected to one end of the transmission rod, and the transmission rod is hollow; Four hollow strips are arranged on the wall surface of the transmission rod, and the four hollow strips are evenly arranged along the circumference of the transmission rod. The length of the hollow strips is slightly smaller than the length of the transmission rod, so that the two ends of the hollow strips do not extend to the two ends of the transmission rod.

2. The dynamic mechanical properties testing device for cover glass according to claim 1, characterized in that: The impact rod is a solid cylinder, and both ends of the impact rod are smooth and flat circular end faces. The impact rod can withstand the compressed air acceleration of the air cannon, so that the head end face of the impact rod hits the waveform shaper at the tail of the incident rod.

3. The dynamic mechanical properties testing device for cover glass according to claim 2, characterized in that: The incident rod is a solid cylinder with a horizontal central axis; the tail of the incident rod is a smooth and flat circular end surface, the head is wedge-shaped, a striking part is arranged at the center of the wedge-shaped head, the tail of the striking part is connected to the incident rod and is integrally formed, and the head of the striking part protrudes outward and is a section of an arc surface; The central axis of the arc surface is horizontal and perpendicular to the central axis of the incident rod, the central axis of the arc surface passes through the central axis of the incident rod, and the length of the central axis of the arc surface is equal to the diameter of the end face of the incident rod; The arc of the arc surface of the impact portion is 2.09-3.84 rad.

4. The dynamic mechanical properties testing device for cover glass according to claim 3, characterized in that: The front side of the clamping device is vertical, and includes a bottom surface, a supporting surface, a supporting portion and an outer edge surface from the inside to the outside. The bottom surface, the supporting surface and the outer edge surface are all smooth and flat planes. The bottom surface is located in the middle of the clamping device. A supporting surface is respectively provided on the upper and lower sides of the bottom surface. The included angle between the supporting surface and the bottom surface is an obtuse angle. One side of the supporting portion is connected to the supporting surface, and the other side is connected to the outer edge surface. The other side of the outer edge surface is connected to the top surface or the bottom surface of the clamping device. The upper and lower supporting portions provide double-point support for the cover glass.

5. The dynamic mechanical properties testing device for cover glass according to claim 4, characterized in that: The tail of the support part is adjacent to the main body of the clamping device, and the head part protrudes toward the incident rod and is a section of an arc surface. The central axis of the arc surface of the support part is parallel to the central axis of the arc surface of the impact part, and the length of the central axis of the arc surface of the support part is equal to the width of the clamping device; The arc angle of the arc surface of the support portion is 2.09-3.84 rad.

6. The dynamic mechanical properties testing device for cover glass according to claim 5, characterized in that: The impact rod, incident rod, clamping device and transmission rod are made of the same material, which is high-strength aluminum alloy; the impact rod, incident rod and transmission rod have the same outer diameter, and the central axes of the three are on the same horizontal line, and the centers of the cover glass and the clamping device are also on this horizontal line.

7. A testing method, using the dynamic mechanical properties testing device for cover glass according to claim 6, characterized in that: The following steps are involved: (1) Arrange the force-applying device, the impact rod, the waveform shaper, the incident rod, the clamping device, and the transmission rod horizontally along the same axis in sequence; adhere strain gauges to the middle of the outer side surface of the incident rod and the middle of the outer side surface of the transmission rod respectively, and connect the strain gauges to the data analysis device; (2) The cover glass is placed between the incident rod and the clamping device. The incident rod and the clamping device apply a pre-tightening force to the cover glass so that the cover glass does not fall off; (3) The high-pressure gas of the force-applying device drives the impact rod, so that the impact rod hits the waveform shaper of the incident rod, generating a compression stress wave, which propagates in the incident rod to the cover glass and performs impact loading on the cover glass, generating a reflection wave that is reflected back to the incident rod, and at the same time generating a transmission wave that propagates along the transmission rod; (4) The voltage data is collected and recorded by the strain gauges of the incident rod and the transmitted rod to obtain the original waveform. The dynamic bending stress curves and loading speed time history curves of the incident rod and the transmitted rod are then analyzed and obtained to obtain the dynamic bending strength.

8. The testing method according to claim 7, characterized in that: In step (1), the transmission rod is supported by two brackets, the clamping device is also supported along with the transmission rod, the incident rod is supported by two brackets, the waveform shaper is also supported along with the incident rod, and the impact rod is supported by two brackets; In step (2), the incident rod is tied to the bracket of the incident rod close to the cover glass with a rubber band to provide a force in the direction of the cover glass for the incident rod; the transmission rod is tied to the bracket of the transmission rod close to the cover glass with a rubber band to provide a force in the direction of the cover glass for the transmission rod, so that the incident rod and the transmission rod can exert forces in opposite directions on the cover glass, thereby clamping the cover glass.

9. The testing method according to claim 8, characterized in that: In step (4), the voltage data is the voltage signal measured by the two strain gauges, and then the original waveform is obtained; through the bridge theory, the voltage signal can be converted into the strain time history data of the incident wave , strain time history data of reflected wave Strain time history data of the transmitted wave ; Then calculate the bending load F(t) and bending stress of the transmission rod and the incident rod and loading speed v(t), the dynamic bending stress curve and the loading speed time curve are obtained; the bending stress at different times can be obtained according to the dynamic bending stress curve, and the highest point of the dynamic bending stress curve is the bending strength.

10. The testing method according to claim 9, characterized in that: The bending load obtained from the incident and reflected waves is given by the following formula: ; Where, t is time, μs; E I is the elastic modulus of the incident rod, MPa; A I is the cross-sectional area of ​​the incident rod, mm 2 ; The bending load obtained from the transmitted wave is determined by the following formula: ; Among them, E T is the elastic modulus of the transmission rod, MPa; A T is the cross-sectional area of ​​the transmission rod, mm 2 ; The unit of the above bending load is N; The bending stress resulting from the incident and reflected waves is determined by the following formula: ; The bending stress obtained from the transmitted wave is determined by the following formula: ; Wherein, L is the span of the cover glass, that is, the distance between the two lines of the cover glass supported by the two supporting parts, mm; b is the width of the cover glass, mm; h is the height of the cover glass, mm; the units of the above bending stresses are all MPa; Dynamic bending stress balance factor β is expressed as follows: ; in, and are the bending stress values ​​corresponding to the dynamic bending stress curve obtained by using the incident wave and reflected wave data and the dynamic bending stress curve obtained by using the transmitted wave data at the same time; If during the loading process, β is always less than 10% from the time when the value of the bending stress of any dynamic bending stress curve reaches 40% of the peak value of the bending stress of the corresponding curve as the starting point to the peak value of any dynamic bending stress curve as the end point, then it is considered that the loads between the incident rod, the transmitted rod and the sample remain in a balanced state during the loading process.

Citation Information

Patent Citations

  • Impact tension testing apparatus

    CN102890035A

  • Material dynamic fracture tenacity measuring device based on Hopkinson bar

    CN108918299A