A method and system for preparing a cable with a shielding layer
By monitoring and adjusting the nitrogen filling speed in real time during the cable preparation process, the problem of unstable cable impedance and capacitance values caused by unbalanced stress in the shielding layer is solved, and the signal transmission stability and electromagnetic shielding effect of the cable are improved.
Patent Information
- Application Number
- CN202411117035.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-15
AI Technical Summary
When preparing cables with the existing technology, the unbalanced twisting stress of the shielding layer causes electromagnetic interference and unstable cable impedance and capacitance values, which cannot effectively solve the signal stability problem of cables in high-speed transmission and information exchange.
By filling the plastic melt with nitrogen and co-extruded with nitrogen to cover the wire core, the untwisting and unwinding machine and the wrapping machine are used for stress monitoring and adjustment, and the nitrogen filling speed is adjusted in real time through changes in capacitance to ensure the thickness of the foam layer and the coating The tape tension is balanced, thus stabilizing the cable impedance and capacitance values.
The stability of cable impedance and capacitance values is improved, ensuring the reliability of signal transmission and electromagnetic shielding effect, especially significantly improving communication performance in long-distance transmission.
Smart Images

Figure CN118645317B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of intelligent manufacturing equipment, in particular to the field of cable preparation technology, and specifically to a method and system for preparing a cable with a shielding layer. Background Art
[0002] The shielding layer of a cable is a layer of semi-conductive material that covers the surface of the conductor or insulation layer and is used to maintain the same potential as the shielded part and make good contact with it. In power cables, a magnetic field is generated around due to the large current passing through. By adding a shielding layer, this electromagnetic field can be effectively shielded inside the cable. In the process of preparing the cable, the shielding layer is usually composed of a metal mesh braided layer, which is wrapped around the outer layer of the wire core. This structural design is designed to reduce the impact of external electromagnetic fields on power or communication lines and ensure that signals can be transmitted stably. At the same time, the metal mesh braided layer can also effectively prevent the line from radiating electromagnetic energy outward, thereby reducing electromagnetic interference to other devices and systems. These functions are essential to ensure the high performance and reliability of cables in modern high-speed transmission and information exchange applications.
[0003] The shielding layer is generally formed by wrapping the cable core with aluminum foil through a wrapping machine. When the cable core is wrapped with aluminum foil on the wrapping machine, the twisting stress will inevitably be transferred to the process before the wrapping, resulting in a gradual increase in the twisting stress of the coated cable core. This unbalanced twisting stress will cause local stress concentration in the formed shielding layer. The electromagnetic interference generated by the stress concentration of the shielding layer will cause abnormal cable impedance and unstable capacitance, so that the final produced cable meets the technical standards in terms of transmission bandwidth, transmission rate and data transmission stability; the invention patent with Chinese patent publication number CN118155955A, although considering the adaptive compensation of the wrapping tension of the wrapping machine to adapt to the continuous stress imbalance, thereby reducing the electric field concentration of the cable, it only reduces the change of mechanical and physical properties on the cable segment to solve the electromagnetic interference problem caused by the electric field concentration. When the wrapping tension of some cable segments is significantly greater than that of other cable segments, the impedance and capacitance of the cable in this part are still unstable, and the problem of stabilizing the capacitance value of the cable is not solved. Summary of the invention
[0004] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a cable with a shielding layer is provided, the method comprising the following steps:
[0005] S100, drawing a wire core by a wire drawing machine, filling nitrogen into a plastic melt, and co-extruding the plastic melt and nitrogen onto the surface of the wire core to obtain an insulated wire core;
[0006] S200, arranging a plurality of insulated wire cores in parallel, and using an active detwisting pay-off machine to detwist and pay off the insulated wire cores to obtain a detwisted wire bundle;
[0007] S300, in the process of untwisting and unwinding, after obtaining the stress value of the untwisted wire bundle, the insulating wire core is fully covered with aluminum foil by a wrapping machine to form a cable core;
[0008] S400, weaving a shielding layer outside the cable core by a braiding machine, and extruding and coating by an extruder to obtain a molded cable, adjusting the nitrogen filling speed in real time according to the change of the electric capacity, and going to step S100 each time the nitrogen filling speed is adjusted until the molded cable is prepared;
[0009] In S400, the method for adjusting the nitrogen filling speed in real time through the change of capacitance is specifically as follows: the steady-state time is monitored according to the stress value. If the steady-state time is obtained, starting from the current moment, after the steady-state time has passed, the newly obtained formed cable within the steady-state time is pulled into the capacitance tester to collect the capacitance; the nitrogen filling speed is dynamically adjusted according to the change of capacitance.
[0010] Further, in S100, the method of filling nitrogen into a plastic melt and co-extruding the plastic melt and the nitrogen onto the surface of the wire core to obtain an insulated wire core includes: preheating the wire core (preheating to a temperature between 130°C and 145°C); placing polyolefin plastic particles into a fluoroplastic extruder for plasticization and melting, allowing the polyolefin plastic particles to melt by heat in the extruder to obtain a plastic melt, filling nitrogen into the screw chamber of the extruder, and under the action of pressure, the plastic melt and the filled nitrogen are co-extruded and coated onto the surface of the wire core to obtain an insulated wire core coated with a foaming layer.
[0011] Further, in S100, the wire core is any one of a copper wire, a copper-clad aluminum wire, an aluminum wire, a copper alloy wire, and an aluminum alloy wire.
[0012] In S200 , a plurality of roots means two or more roots.
[0013] Further, in S300, the method for obtaining the stress value of the detwisted wire harness is: obtaining the stress value of the detwisted wire harness by using a wireless stress sensor or a fiber grating stress sensor.
[0014] Since the thickness of the foaming layer filled with nitrogen in the cable will directly cause the cable impedance and capacitance value of the cable to change, and the change of the tape tension of the wrapping machine will also cause the cable stress to change, thereby indirectly affecting the cable impedance and capacitance value, the bubbles and tape tension of the foaming layer generated by the nitrogen filling in the cable will affect the cable impedance and capacitance value, and the final cable impedance and capacitance value are finally generated after the two are balanced. Therefore, to adjust the nitrogen filling speed, it is necessary to first accurately locate the timing when the thickness of the foaming layer and the tape tension are balanced according to the change of the stress value of the back-twisted wire harness, and ensure the stability of the cable impedance and capacitance value according to this timing, so as to determine how to adjust the nitrogen filling speed. Therefore, the present invention provides the following method to locate the steady-state time period when the thickness of the foaming layer and the tape tension are balanced, and the steady-state time period is used as the steady-state duration for positioning, specifically:
[0015] Further, in S400, the method for monitoring the steady-state duration according to the stress value specifically includes:
[0016] Starting from the first detwisting and pay-off, all the acquired stress values of the detwisting harness are sorted in the order of acquisition time, and then each stress value is searched in sequence: if the current stress value is less than the previous stress value and less than the next stress value, the current stress value is marked as the preceding steady-state moment, and the search for each stress value starts again in sequence from the preceding steady-state moment. If the current stress value is less than the previous stress value and less than the next stress value, the current stress value is marked as the post-steady-state moment, and the duration between the preceding steady-state moment and the post-steady-state moment is the steady-state duration.
[0017] The above method can quickly locate the duration of the local time period with smaller torsional stress during the first period of time after the start of manufacturing of the cable through the stress value at two local low positions. The reason why this time period can reflect the balance between the thickness of the foaming layer and the tension of the wrapping tape is that when the outer edge of the foam of the solidified bubbles in the foaming layer is subjected to the lateral force of the wrapping tape tension, the length of the edge of each bubble is relatively similar to that of the regular uniform bubble, so that a geometric pattern similar to a space truss structure with stable force is formed, so that the outer edge of the bubble structure of the solidified foaming layer is transferred to the inner side to bear the force, and can stably withstand loads from all directions; however, since the edge of the nitrogen-filled foam in the foaming layer will randomly produce irregular multiple If a large number of dense small bubbles or local thinning appears in the foaming layer of a certain section of cable, its structure is not a geometric style of a space truss structure with stable force, so it cannot withstand large loads from the outside and the direction of adjacent bubbles. Larger wrapping force (outside of the cable) or stress generated by the twisting line (generated on the inside of the cable, the wrapping force and the stress generated by the twisting line generally need to offset each other) can easily cause the fragile foam edge of the foaming layer to collapse locally (the foam edge of the foaming layer of the cable section is compressed and collapsed by the external load), resulting in a small stress change in the cable section generated in this time period after the local collapse, resulting in the inability to identify the steady-state duration in this time period. The present invention proposes the following preferred method for monitoring the steady-state duration:
[0018] Preferably, in S400, the method for monitoring the steady-state duration according to the stress value specifically includes:
[0019] All the stress values of the back-twisted harness obtained are sequentially formed into a stress sequence in the order of acquisition time; the minimum value in the stress sequence is recorded as StrLow, and the average value is recorded as StrMean; all the stress values in the stress sequence that are greater than StrLow and less than StrMean constitute a low-stable stress sequence (the low-stable stress sequence is because the fragile foam edge of the foaming layer produces local collapse, so the structure with less stress is not the stress value of the space truss structure with stable force. In the low-stable stress sequence, the foaming layer of the cable segment corresponding to these time periods has a small stress change after local collapse); sequentially obtain the interval time length corresponding to the acquisition time between each adjacent stress value in the low-stable stress sequence as the low-stable time sequence UnSTime;
[0020] The stable end time VirtualTime is predicted according to the following formula:
[0021] ;
[0022] StartTime is the acquisition time corresponding to the first stress value less than StrMean among the stress values in the stress sequence;
[0023] UnSTime(i) is the length of the i-th interval in UnSTime; M is the number of intervals in UnSTime; i is the sequence number of the interval; Portion(i) is the stable potential ratio of the i-th interval in UnSTime,
[0024] Portion(i)=StartUnTime(i) / UnSTimeMean;
[0025] UnSTimeMean is the average length of each interval in UnSTime;
[0026] StartUnTime(i) is the stress stability duration in the time interval corresponding to UnSTime(i). The method for obtaining the value of StartUnTime(i) is as follows: obtain the stress values in the time interval corresponding to UnSTime(i) in the stress sequence to form the first subsequence in sequence, and make judgments from the stress value after the smallest stress value S1 in the first subsequence: if there is a stress value that is less than the mean value of the low stable stress sequence for the first time, mark the stress value as S2; the time interval between the acquisition times corresponding to S1 and S2 is StartUnTime(i);
[0027] The time for obtaining the last stress value less than StrMean in the stress sequence is EndTime, and the time length between EndTime and the stable end time VirtualTime is the steady-state duration.
[0028] The stable end time VirtualTime is an estimated time calculated based on the changing trend of the collected stress values between each cable segment. VirtualTime can estimate the end time of the continuous small stress change of the foaming layer of the cable segment after local collapse. The stable potential estimation ratio Portion(i) is the ratio between the short time that can be monitored within the short time of the i-th interval time length in UnSTime and the overall mean value of UnSTime. It can accurately reflect the proportion of the local collapse maintenance time of the foaming layer within this short time to the overall mean value, so that the subsequent calculated stable end time can be based on the change of the historical collapse trend of the foaming layer. When the stress change of the cable segment is small and cannot be detected after the local collapse, the steady-state time period, i.e., the steady-state duration, when the thickness of the foaming layer and the tension of the wrapping tape are balanced can be accurately located by estimation.
[0029] Further, in S400, the method for dynamically adjusting the nitrogen charging speed according to the change of the electric capacity specifically includes:
[0030] The collected capacitances are sequentially formed into a sequence CapaList; the maximum value in the sequence CapaList is MaxCap, the average value is MeanCap, the minimum value is MinCap, and the most recently collected capacitance is CurrentCap;
[0031] Among all the capacitance values collected within the steady-state duration after the collection moment corresponding to MaxCap in the marker sequence CapaList, the capacitance value with a capacitance less than CurrentCap is the reference steady-state increase capacitance; the value with the smallest difference with CurrentCap among the reference steady-state increase capacitances is NearCap1, and the absolute value of the difference between NearCap1 and CurrentCap after rounding is IndiUp;
[0032] The capacitance value with a capacitance greater than CurrentCap among all the capacitance values collected within the steady-state duration after the collection moment corresponding to MinCap in the marker sequence CapaList is the reference steady-state reduced capacitance; the value with the smallest difference with CurrentCap among all the reference steady-state reduced capacitances is NearCap2; the absolute value of the difference between NearCap2 and CurrentCap after rounding is IndiDo;
[0033] When IndiUp>IndiDo, the current nitrogen filling speed is reduced within a steady-state duration; (the reason for the instability of the capacitance at this time is that the increasing trend of the current capacitance in the reference steady-state increasing capacitance is significantly greater than the decreasing trend of the reference steady-state decreasing capacitance, and the foam structure of the foaming layer is mainly large foam, so the nitrogen filling speed needs to be reduced to reduce the generation of large foam);
[0034] When IndiUp<IndiDo, the current nitrogen filling speed is increased within a steady-state duration; (the reason for the instability of the capacitance at this time is that the increasing trend of the current capacitance in the reference steady-state increasing capacitance is significantly smaller than the decreasing trend of the reference steady-state decreasing capacitance, and the foam structure of the foaming layer is mainly small foams, so the nitrogen filling speed needs to be increased to increase the generation of large foams);
[0035] When IndiUp is equal to IndiDo, the current nitrogen filling pressure is maintained.
[0036] The reference steady-state increasing capacitance and the reference steady-state decreasing capacitance are capacitance values that are screened out from the capacitances that are continuously and stably increasing and continuously and stably decreasing in the steady-state time period when the thickness of the foaming layer and the tension of the wrapping tape are balanced after the maximum value and the minimum value, respectively, and have a variation trend similar to the capacitance collected most recently. Note: In order to screen out capacitance values that are similar to the variation trend of the capacitance collected most recently in the capacitances that are continuously and stably increasing, in the steady-state time period that continues after the MaxCap acquisition moment, the capacitance value will show high outlier performance, so the reference steady-state increasing capacitance selects all capacitance values that are less than the CurrentCap with stable growth; on the contrary, in the steady-state time period that continues after the MinCap acquisition moment, the capacitance value will show low outlier performance, so the reference steady-state decreasing capacitance selects all capacitance values that are greater than the CurrentCap with stable growth.
[0037] Preferably, in S400, the following steps are included:
[0038] The method of reducing the current nitrogen filling speed within a steady-state period is as follows: within a steady-state period, reduce the current nitrogen filling speed into the screw chamber of the extruder by 0.03 to 0.08 m / s. 3 / h, so that the nitrogen pressure in the screw chamber of the extruder is maintained in the pressure range of 1 to 1.5 kPa higher than the atmospheric pressure;
[0039] The method for increasing the current nitrogen filling speed within a steady-state period is as follows: within a steady-state period, increase the current nitrogen filling speed into the screw chamber of the extruder by 0.03 to 0.08 m / s. 3 / h, so that the nitrogen pressure in the screw chamber of the extruder is maintained in the pressure range of 2.5 to 3 kPa higher than the atmospheric pressure;
[0040] The specific method of maintaining the current nitrogen filling pressure is: 0.1 ~ 0.25m 3 The nitrogen is filled into the screw chamber of the extruder at a nitrogen filling rate of / h until the pressure in the screw chamber is within the range of 1.5 to 2.5 kPa of the atmospheric pressure.
[0041] Among them, by adjusting the nitrogen filling speed, the bubbles in the foaming layer of the subsequently produced cable are made relatively uniform, forming a geometric style similar to a space truss structure with stable force, so that the outer edge of the bubble structure after the foaming layer solidifies is transferred to the inner side to bear the force, and can stably withstand the loads from the inside and outside directions in the subsequent twisting and wrapping processes, thereby increasing the stability of the impedance and capacitance values of the prepared cable.
[0042] Further, in S400, the method of obtaining a molded cable by extrusion coating with an extruder is: melt the plastic with an extruder to obtain plastic liquid, extrude the plastic liquid and coat the outer layer of the shielding layer woven outside the cable core, and obtain the molded cable after cooling.
[0043] Further, in S400, the method of braiding the shielding layer outside the cable core by a braiding machine is specifically: using a 24-spindle rope braiding machine to cross-weave metal wires outside the cable core to form a mesh shielding layer of metal wires.
[0044] Preferably, after the shaped cable is prepared, the shaped cable is rolled up by a wire take-up machine to obtain a cable roll.
[0045] Furthermore, in S400, the capacitance tester is an online underwater capacitance tester, which is used for online measurement of cable capacitance. During the extrusion process of the cable, the online underwater capacitance tester monitors the capacitance in real time. The online underwater capacitance tester is placed in a cooling water tank, and the cable passes through the inside of the online underwater capacitance tester. The conductor in the cable and the insulating surface form a cylindrical capacitor, and its capacitance data is transmitted to the host through a converter, and the host then processes and displays the data.
[0046] Preferably, in S400, the capacitance tester is a Fuguang FK-630X online underwater capacitance tester.
[0047] Preferably, in S400, the cable traction is performed by a traction machine.
[0048] The present invention also provides a cable preparation system with a shielding layer, the system comprising: a processor, a memory, and a computer program stored in the memory and running on the processor; when the processor executes the computer program, the steps in a cable preparation method with a shielding layer are implemented. The cable preparation system with a shielding layer can be run in computing devices such as desktop computers, handheld computers, and cloud data centers. The executable system may include but is not limited to: a processor, a memory, and a server cluster.
[0049] As described above, the method and system for preparing a cable with a shielding layer described in the present invention have the following beneficial effects: it can accurately calculate the steady-state duration for measuring the stability of the capacitance value during the cable drawing process. And by adjusting the nitrogen filling speed, the bubbles in the foaming layer of the subsequently produced cable are relatively uniform, forming a geometric pattern similar to a space truss structure with stable force, so that the outer edge of the bubble structure after the foaming layer solidifies is transferred to the inner side to bear the force, and can stably withstand the load from the inner and outer directions in the subsequent twisting and wrapping process, thereby increasing the stability of the prepared cable impedance and capacitance value; and when the tape tension of some cable sections is significantly greater than that of other cable sections, the impedance and capacitance values of the cable in this section can still be stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1Shown is a flow chart of a method for preparing a cable with a shielding layer. DETAILED DESCRIPTION
[0051] The following will be combined with the embodiments and drawings to clearly and completely describe the concept, specific structure and technical effects of the present invention, so as to fully understand the purpose, scheme and effect of the present invention. It should be noted that the embodiments and features in the embodiments of this application can be combined with each other without conflict.
[0052] like Figure 1 The flowchart of the method for preparing a cable with a shielding layer according to the present invention is shown below. Figure 1 A method for preparing a cable with a shielding layer according to an embodiment of the present invention is described below.
[0053] Embodiment 1:
[0054] The present invention provides a method for preparing a cable with a shielding layer, the method specifically comprising the following steps:
[0055] S100, drawing a wire core by a wire drawing machine, filling nitrogen into a plastic melt, and co-extruding the plastic melt and nitrogen onto the surface of the wire core to obtain an insulated wire core;
[0056] S200, arranging two insulated wire cores in parallel, and using an active detwisting pay-off machine to detwist and pay off the insulated wire cores to obtain a detwisted wire bundle;
[0057] S300, in the process of untwisting and unwinding, after obtaining the stress value of the untwisted wire harness, a multi-head wrapping machine of an Omron CJ1W-MCH71 motion controller is used to fully wrap the insulated wire core with aluminum foil to form a cable core;
[0058] S400, weaving a shielding layer on the outside of the cable core by a 24-spindle rope braiding machine, and extruding and coating by an extruder to obtain a molded cable, adjusting the nitrogen filling speed in real time according to the change of the electric capacity, and going to step S100 each time the nitrogen filling speed is adjusted until the molded cable is prepared;
[0059] In S400, the method for adjusting the nitrogen filling speed in real time through the change of capacitance is specifically as follows: the steady-state time is monitored according to the stress value. If the steady-state time is obtained, starting from the current moment, after the steady-state time has passed, the newly obtained formed cable within the steady-state time will be pulled into the Fuguang FK-630X online water capacitance detector to collect the capacitance; the nitrogen filling speed is dynamically adjusted according to the change of capacitance.
[0060] Further, in S100, the method of filling nitrogen into the plastic melt and co-extruding the plastic melt and nitrogen onto the surface of the wire core to obtain an insulated wire core includes: preheating the wire core to a temperature of 145°C; placing polyolefin plastic particles into a fluoroplastic extruder for plasticization and melting, allowing the polyolefin plastic particles to melt in the extruder under heat to obtain a plastic melt, filling nitrogen into the screw chamber of the extruder, and under pressure, the plastic melt and the charged nitrogen are co-extruded and coated onto the surface of the wire core to obtain an insulated wire core coated with a foaming layer. Wherein, the wire core is a copper-clad aluminum wire core.
[0061] The back-twist rate of the back-twist machine is set to 15%.
[0062] Further, in S300, the method for obtaining the stress value of the detwisted wire harness is: obtaining the stress value of the detwisted wire harness by using a fiber Bragg grating stress sensor.
[0063] Further, in S400, the method for monitoring the steady-state duration according to the stress value specifically includes:
[0064] Starting from the first detwisting and pay-off, all the acquired stress values of the detwisting harness are sorted in the order of acquisition time, and then each stress value is searched in sequence: if the current stress value is less than the previous stress value and less than the next stress value, the current stress value is marked as the preceding steady-state moment, and the search for each stress value starts again in sequence from the preceding steady-state moment. If the current stress value is less than the previous stress value and less than the next stress value, the current stress value is marked as the post-steady-state moment, and the duration between the preceding steady-state moment and the post-steady-state moment is the steady-state duration.
[0065] Further, in S400, the method for dynamically adjusting the nitrogen charging speed according to the change of the electric capacity specifically includes:
[0066] The collected capacitances are sequentially formed into a sequence CapaList; the maximum value in the sequence CapaList is MaxCap, the average value is MeanCap, the minimum value is MinCap, and the most recently collected capacitance is CurrentCap;
[0067] Among all the capacitance values collected within the steady-state duration after the collection moment corresponding to MaxCap in the marker sequence CapaList, the capacitance value with a capacitance less than CurrentCap is the reference steady-state increase capacitance; the value with the smallest difference with CurrentCap among the reference steady-state increase capacitances is NearCap1, and the absolute value of the difference between NearCap1 and CurrentCap after rounding is IndiUp;
[0068] The capacitance value with a capacitance greater than CurrentCap among all the capacitance values collected within the steady-state duration after the collection moment corresponding to MinCap in the marker sequence CapaList is the reference steady-state reduced capacitance; the value with the smallest difference with CurrentCap among all the reference steady-state reduced capacitances is NearCap2; the absolute value of the difference between NearCap2 and CurrentCap after rounding is IndiDo;
[0069] When IndiUp>IndiDo, the current nitrogen filling speed is reduced within a steady state period. Specifically, within a steady state period, the current nitrogen filling speed into the screw chamber of the extruder is reduced by 0.08m 3 / h, so that the nitrogen pressure in the screw chamber of the extruder is maintained in the pressure range of 1 to 1.5 kPa higher than the atmospheric pressure;
[0070] When IndiUp<IndiDo, the current nitrogen filling speed is increased within a steady-state period. Specifically, within a steady-state period, the current nitrogen filling speed into the screw chamber of the extruder is increased by 0.08m 3 / h, so that the nitrogen pressure in the screw chamber of the extruder is maintained in the pressure range of 2.5 to 3 kPa higher than the atmospheric pressure;
[0071] When IndiUp is equal to IndiDo, maintain the current nitrogen filling pressure, specifically: 0.1m 3 The nitrogen is filled into the screw chamber of the extruder at a nitrogen filling rate of / h until the pressure in the screw chamber is within the range of 1.5 to 2.5 kPa of the atmospheric pressure.
[0072] Further, in S400, the method of obtaining a molded cable by extrusion coating with an extruder is: melt the plastic with an extruder to obtain plastic liquid, extrude the plastic liquid and coat the outer layer of the shielding layer woven outside the cable core, and obtain the molded cable after cooling.
[0073] Embodiment 2:
[0074] Example 2 is based on Example 1, and the method of monitoring the steady-state duration according to the stress value is replaced by the following method:
[0075] Preferably, in S400, the method of monitoring the steady-state duration according to the stress value is replaced by:
[0076] All the stress values of the detwisted harness obtained are sequentially collected in the order of acquisition time to form a stress sequence; the minimum value in the stress sequence is recorded as StrLow and the average value is recorded as StrMean; all stress values in the stress sequence that are greater than StrLow and less than StrMean form a low-stable stress sequence; the interval lengths of the acquisition times corresponding to each adjacent stress value in the low-stable stress sequence are sequentially obtained as a low-stable time sequence UnSTime;
[0077] The stable end time VirtualTime is predicted according to the following formula:
[0078] ;
[0079] StartTime is the acquisition time corresponding to the first stress value less than StrMean among the stress values in the stress sequence;
[0080] UnSTime(i) is the length of the i-th interval in UnSTime; M is the number of intervals in UnSTime; i is the sequence number of the interval; Portion(i) is the stable potential ratio of the i-th interval in UnSTime,
[0081] Portion(i)=StartUnTime(i) / UnSTimeMean;
[0082] UnSTimeMean is the average length of each interval in UnSTime;
[0083] StartUnTime(i) is the stress stability duration in the time interval corresponding to UnSTime(i). The method for obtaining the value of StartUnTime(i) is as follows: obtain the stress values in the time interval corresponding to UnSTime(i) in the stress sequence to form the first subsequence in sequence, and make judgments from the stress value after the smallest stress value S1 in the first subsequence: if there is a stress value that is less than the mean value of the low stable stress sequence for the first time, mark the stress value as S2; the time interval between the acquisition times corresponding to S1 and S2 is StartUnTime(i);
[0084] The time for obtaining the last stress value less than StrMean in the stress sequence is EndTime, and the time length between EndTime and the stable end time VirtualTime is the steady-state duration.
[0085] Comparative Example:
[0086] A method for preparing an unshielded twisted pair cable comprises the following steps:
[0087] S1. Wire drawing: Select copper-clad aluminum wire and use a wire drawing machine to make a wire core conductor. Each single wire conductor is wrapped with an insulating layer.
[0088] S2. Twisted pair: Two wire cores form a set of twisted wire pairs, twisted together in a twisted pair structure;
[0089] S3. Cabling: Cabling is done by pre-twisting cabling machine with a twisting rate of 15%;
[0090] S4. Sheath: The plastic is melted by an extruder to obtain plastic liquid, which is then squeezed out onto the cable and covered with a sheath to obtain a molded cable.
[0091] The formed cables prepared in Example 1, Example 2 and the comparative example were cut into three groups of cables with lengths of 50 meters, 100 meters and 500 meters, respectively, namely a 50-meter cable group, a 100-meter cable group and a 500-meter cable group;
[0092] Note: Since the maximum effective transmission distance of the twisted pair cable is 100 meters, the 500-meter cable group here is a 500-meter cable divided into five 100-meter cables, and the five 100-meter cables are connected into five network segments through four UTP3-VER01-POE repeaters in turn to form the 500-meter cable groups of Example 1, Example 2 and the comparative example.
[0093] The three sets of cables of 50 meters, 100 meters, and 500 meters in Example 1, Example 2, and Comparative Example were respectively equipped with 100M Ethernet ports, and communication performance tests were performed using a vector network analyzer MS4624D at a frequency of 100MHz in accordance with the requirements of Ethernet standard 802.3;
[0094] The test data obtained after testing the 50-meter cable set are:
[0095] The communication performance data of Example 1 are: return loss 26.8dB, insertion loss 1.0dB, near-end crosstalk 26.4dB;
[0096] The communication performance data of Example 2 is: return loss 32.5dB, insertion loss 0.4dB, near-end crosstalk 22.6dB;
[0097] The communication performance data of the comparative example are: return loss 17.7dB, insertion loss 2.2dB, and near-end crosstalk 28.6dB.
[0098] The test data obtained after testing the 100-meter cable set is:
[0099] The communication performance data of Example 1 are: return loss 24.5dB, insertion loss 1.1dB, near-end crosstalk 28.7dB;
[0100] The communication performance data of Example 2 is: return loss 30.7dB, insertion loss 0.5dB, near-end crosstalk 24.4dB;
[0101] The communication performance data of the comparative example are: return loss 14.4dB, insertion loss 2.5dB, and near-end crosstalk 30.3dB.
[0102] The test data obtained after testing the 500-meter cable set are:
[0103] The communication performance data of Example 1 are: return loss 19.1dB, insertion loss 9.5dB, near-end crosstalk 31.1dB;
[0104] The communication performance data of Example 2 are: return loss 25.9dB, insertion loss 7.2dB, near-end crosstalk 29.2dB;
[0105] The communication performance data of the comparative example are: return loss 10.5dB, insertion loss 16.9dB, and near-end crosstalk 35.3dB.
[0106] According to the above test results, the communication performance of the finished cable prepared according to Example 1 and Example 2 is better than that of the formed cable prepared according to the comparative example, and the signal transmission stability is good. Since the cables of Example 1 and Example 2 are subsequently nitrogen-filled and controlled according to the duration of the capacitance value maintaining stability during the cable drawing process, the longer the cable, the more obvious the data superiority is compared with the comparative example cable, especially the comparative example 2 can accurately locate the steady-state time period when the thickness of the foaming layer and the tension of the wrapping tape are balanced by estimation, that is, the steady-state duration, so that the outer edge of the bubble structure after the foaming layer solidifies is transferred to the inner side to bear the force, and can stably withstand the load from the inner and outer directions in the subsequent twisting and wrapping process, thereby increasing the stability of the prepared cable impedance and capacitance value, so the stability of the return loss of the comparative example 2 in the long-distance cable is significantly better than that of the comparative example. Note: Since the 500-meter cable group is composed of 5 100-meter cable segments connected by 4 repeaters, the insertion loss of the 500-meter cable group increases significantly.
[0107] Among them, return loss is the reflection caused by impedance mismatch in the cable link. The calculated result of return loss is always a positive number. The larger the value, the smaller the signal reflection, which is more conducive to signal transmission. The smaller the insertion loss value, the better the performance (the maximum allowable insertion loss limit of 100MHz Category 5e cable is 22dB). The smaller the near-end crosstalk (NEXT) value, the better the performance. Due to the existence of line loss, the impact on the far-end crosstalk (FEXT) value is small, so the vector network analyzer only measures the near-end crosstalk (NEXT).
[0108] The present invention also provides a cable preparation system with a shielding layer, the system comprising: a processor, a memory, and a computer program stored in the memory and running on the processor; when the processor executes the computer program, the steps in a cable preparation method with a shielding layer are implemented. The cable preparation system with a shielding layer can be run in computing devices such as desktop computers, handheld computers, and cloud data centers. The executable system may include but is not limited to: a processor, a memory, and a server cluster.
[0109] Those skilled in the art will appreciate that the example described is merely an example of a cable preparation system with a shielding layer and does not constitute a limitation on a cable preparation system with a shielding layer. The system may include more or fewer components than the example, or a combination of certain components, or different components. For example, the cable preparation system with a shielding layer may also include input and output devices, network access devices, buses, etc.
[0110] The processor may be a central processing unit (CPU), or other general-purpose processors, digital signal processors (DSP), application-specific integrated circuits (ASIC), field-programmable gate arrays (FPGA) or other programmable logic devices, discrete component gate circuits or transistor logic devices, discrete hardware components, etc. The general-purpose processor may be a microprocessor or any conventional processor, etc. The processor is the control center of the cable preparation system with a shielding layer, and uses various interfaces and lines to connect the various sub-areas of the entire cable preparation system with a shielding layer.
[0111] The memory can be used to store the computer program and / or module, and the processor realizes various functions of the cable preparation method and system with a shielding layer by running or executing the computer program and / or module stored in the memory and calling the data stored in the memory. The memory can mainly include a program storage area and a data storage area, wherein the memory can include a high-speed random access memory and can also include a non-volatile memory, such as a hard disk, a memory, a plug-in hard disk, a smart memory card (Smart Media Card, SMC), a secure digital (SecureDigital, SD) card, a flash card (Flash Card), at least one disk storage device, a flash memory device, or other volatile solid-state storage devices.
[0112] Although the description of the present invention has been quite detailed and has been described in particular with respect to several described embodiments, it is not intended to be limited to any of these details or embodiments or any particular embodiment, so as to effectively cover the intended scope of the present invention. In addition, the present invention is described above with the embodiments foreseeable by the inventors, and its purpose is to provide a useful description, and those non-substantial changes to the present invention that are not currently foreseen may still represent equivalent changes of the present invention.
Claims
1. A method for preparing a cable with a shielding layer, characterized in that: The method comprises the following steps: S100, drawing a wire core by a wire drawing machine, filling nitrogen into a plastic melt, and co-extruding the plastic melt and nitrogen onto the surface of the wire core to obtain an insulated wire core; S200, arranging a plurality of insulated wire cores in parallel, and using an active detwisting pay-off machine to detwist and pay off the insulated wire cores to obtain a detwisted wire bundle; S300, in the process of untwisting and unwinding, after obtaining the stress value of the untwisted wire bundle, the insulating wire core is fully covered with aluminum foil by a wrapping machine to form a cable core; S400, weaving a shielding layer outside the cable core by a braiding machine, and extruding and coating by an extruder to obtain a molded cable, adjusting the nitrogen filling speed in real time according to the change of the electric capacity, and going to step S100 each time the nitrogen filling speed is adjusted until the molded cable is prepared; In S400, the method for adjusting the nitrogen filling speed in real time through the change of capacitance is specifically as follows: the steady-state time is monitored according to the stress value. If the steady-state time is obtained, starting from the current moment, after the steady-state time has passed, the newly obtained formed cable within the steady-state time is pulled into the capacitance tester to collect the capacitance; the nitrogen filling speed is dynamically adjusted according to the change of capacitance.
2. According to the method for preparing a cable with a shielding layer according to claim 1, in S400, the method for monitoring the steady-state duration according to the stress value specifically comprises: Starting from the first detwisting and pay-off, all the acquired stress values of the detwisting harness are sorted in the order of acquisition time, and then each stress value is searched in sequence: if the current stress value is less than the previous stress value and less than the next stress value, the current stress value is marked as the preceding steady-state moment, and the search for each stress value starts again in sequence from the preceding steady-state moment. If the current stress value is less than the previous stress value and less than the next stress value, the current stress value is marked as the post-steady-state moment, and the duration between the preceding steady-state moment and the post-steady-state moment is the steady-state duration.
3. According to the method for preparing a cable with a shielding layer according to claim 2, in S400, the method of monitoring the steady-state duration according to the stress value is replaced by: All the stress values of the detwisted wire harness obtained are sequentially combined into a stress sequence in the order of acquisition time; the minimum value in the stress sequence is recorded as StrLow, and the average value is recorded as StrMean; All stress values in the stress sequence that are greater than StrLow and less than StrMean constitute a low-stable stress sequence; the interval lengths of the acquisition times corresponding to each adjacent stress value in the low-stable stress sequence are obtained in sequence as a low-stable time sequence UnSTime; The stable end time VirtualTime is predicted according to the following formula: ; StartTime is the acquisition time corresponding to the first stress value less than StrMean among the stress values in the stress sequence; UnSTime(i) is the length of the i-th interval in UnSTime; M is the number of intervals in UnSTime; i is the sequence number of the interval; Portion(i) is the stable potential ratio of the i-th interval in UnSTime, Portion(i)=StartUnTime(i) / UnSTimeMean; UnSTimeMean is the average length of each interval in UnSTime; StartUnTime(i) is the stress stability duration in the time interval corresponding to UnSTime(i). The method for obtaining the value of StartUnTime(i) is as follows: obtain the stress values in the time interval corresponding to UnSTime(i) in the stress sequence to form the first subsequence in sequence, and make judgments from the stress value after the smallest stress value S1 in the first subsequence: if there is a stress value that is less than the mean value of the low stable stress sequence for the first time, mark the stress value as S2; the time interval between the acquisition times corresponding to S1 and S2 is StartUnTime(i); The time for obtaining the last stress value less than StrMean in the stress sequence is EndTime, and the time length between EndTime and the stable end time VirtualTime is the steady-state duration.
4. According to the method for preparing a cable with a shielding layer according to claim 1, in S400, the method for dynamically adjusting the nitrogen filling speed according to the change of the capacitance specifically comprises: The collected capacitances are sequentially formed into a sequence CapaList; The maximum value in the sequence CapaList is MaxCap, the average value is MeanCap, the minimum value is MinCap, and the most recently collected capacitance is CurrentCap; Among all the capacitance values collected within the steady-state duration after the collection moment corresponding to MaxCap in the marker sequence CapaList, the capacitance value with a capacitance less than CurrentCap is the reference steady-state increase capacitance; the value with the smallest difference with CurrentCap among the reference steady-state increase capacitances is NearCap1, and the absolute value of the difference between NearCap1 and CurrentCap after rounding is IndiUp; The capacitance value of all the capacitance values collected within the steady-state duration after the collection moment corresponding to MinCap in the marker sequence CapaList, which has a capacitance greater than CurrentCap, is the reference steady-state reduced capacitance; The value with the smallest difference between the reference steady-state reduced capacitance and the CurrentCap is NearCap2; the absolute value of the difference between NearCap2 and CurrentCap after rounding is IndiDo; When IndiUp>IndiDo, the current nitrogen filling speed is reduced within a steady-state period; When IndiUp<IndiDo, the current nitrogen filling speed is increased within a steady-state period; When IndiUp is equal to IndiDo, the current nitrogen filling pressure is maintained.
5. According to the method for preparing a cable with a shielding layer as described in claim 4, the method for reducing the current nitrogen filling speed within a steady-state duration is specifically: within a steady-state duration, reducing the current nitrogen filling speed into the screw chamber of the extruder by 0.03 to 0.08 m / s. 3 / h, so that the nitrogen pressure in the screw chamber of the extruder is maintained in the pressure range of 1 to 1.5 kPa higher than the atmospheric pressure.
6. According to the method for preparing a cable with a shielding layer as claimed in claim 4, the method for increasing the current nitrogen filling speed within a steady-state duration is specifically: within a steady-state duration, increasing the current nitrogen filling speed into the screw chamber of the extruder by 0.03 to 0.08 m / s. 3 / h, so that the nitrogen pressure in the screw chamber of the extruder is maintained in the pressure range of 2.5 to 3 kPa higher than the atmospheric pressure.
7. According to the method for preparing a cable with a shielding layer as claimed in claim 4, the method for maintaining the current nitrogen filling pressure is specifically: 3 Nitrogen is filled into the screw chamber of the extruder at a nitrogen filling rate of / h until the atmospheric pressure in the screw chamber reaches 1.5 kPa.
8. According to the method for preparing a cable with a shielding layer according to claim 1, in S400, the method for obtaining a molded cable by extrusion coating by an extruder is: melting plastic by an extruder to obtain plastic liquid, extruding the plastic liquid and coating the outer layer of the shielding layer woven outside the cable core, and obtaining a molded cable after cooling.
9. A cable preparation system with a shielding layer, characterized in that: The system comprises: a processor, a memory and a computer program stored in the memory and running on the processor; when the processor executes the computer program, the steps in any one of the methods for preparing a cable with a shielding layer in claims 1 to 8 are implemented.