An integrated vacuum internal insulation decorative panel for existing buildings and a preparation method thereof

By using PVC integrated board and modified sepiolite, lignin powder, wood fiber and other materials on the vacuum insulation board, an integrated vacuum insulating decorative board suitable for internal insulation of exterior walls is formed, and the vacuum in the prior art is solved The insulation boards are prone to damage and cost problems in the insulation construction of the exterior wall, achieving low thermal conductivity, water vapor resistance and convenient construction.

CN118650943BActive Publication Date: 2024-11-01SHANDONG CTON ENERGY SAVING TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411129364.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The application of existing vacuum insulation panels in the field of building energy saving is limited, especially in the insulation construction of exterior walls, which are prone to damage, high cost and difficult to apply, and lack suitable construction methods.

Method used

The integrated vacuum insulating decorative panel consisting of PVC integrated board and vacuum insulation board is used to prepare a composite core material by modifying sepiolite, modified lignin powder and wood fibers, and polyethylene film, aluminum foil, and aluminum-plated polyethylene The barrier film bag composed of ethylene terephthalate film and nylon film combines the bonding method of room temperature cured two-component polyurethane glue to form a decorative plate that is resistant to water vapor permeability, low heat conductivity and impact resistance.

Benefits of technology

It realizes vacuum insulated decorative panels that are low-cost, low-thermal conductivity, water vapor permeability, convenient construction and suitable for insulation in exterior walls, improves construction safety and insulation performance, and is suitable for insulation decoration and renovation of old buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

An integrated vacuum internal insulation decorative panel for existing buildings and a preparation method thereof, belonging to the technical field of building insulation, wherein the integrated vacuum internal insulation decorative panel for existing buildings is formed by bonding and compounding a decorative layer and an inner layer, wherein the decorative layer is a PVC integrated panel, the inner layer is a vacuum insulation panel, and the adhesive used for bonding the decorative layer and the inner layer is a two-component polyurethane adhesive that cures at room temperature; the obtained integrated vacuum internal insulation decorative panel for existing buildings has a peel strength of 4.31-4.65 N / 15 mm, a heat sealing strength of 61.35-67.62 N / 15 mm, a wear resistance (mass loss) of 18.94-21.33 mg, a maximum puncture resistance of 22.75-23.43 N, a thermal conductivity of 3.73-4.02 mW / (m·K), and a thermal conductivity of 3.94-4.11 mW / (m·K) after 80 high-temperature water spraying cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an integrated vacuum internal insulation decorative board specially used for existing buildings and a preparation method thereof, belonging to the technical field of building insulation. Background Art

[0002] In recent years, with the development of the global economy, fossil energy such as oil, coal, and natural gas has been used in large quantities, global carbon emissions have increased dramatically, and the greenhouse effect has become prominent, posing a great threat to the human living environment. Therefore, energy conservation and emission reduction, and the development of green and efficient insulation materials are urgent. Since building energy consumption accounts for about one-third of the total social energy consumption, it is of great significance to use safe and efficient insulation materials to reduce building energy consumption.

[0003] Vacuum insulation board, also known as vacuum insulation panel (VIP), is a new type of thermal insulation material with excellent thermal insulation performance and a thermal conductivity as low as 1.5 mW / (m·K). When achieving the same thermal insulation effect, the thickness of the vacuum insulation board is only one-tenth of that of other traditional materials. The use of this material can save a lot of space and is currently the most efficient thermal insulation material. Therefore, the vacuum insulation board is also called a super insulation material.

[0004] Despite the excellent insulation performance of vacuum insulation boards, they have not been widely used in the field of building energy conservation and are still in the initial stage. Most of them are used in the form of external wall insulation. During the construction of external wall insulation, vacuum insulation boards cannot be drilled. At the same time, various bumps and punctures during the construction of the external wall may cause damage to the vacuum insulation board and cause the insulation function to fail, which will increase the difficulty and cost of construction. The use of internal insulation of the external wall is a simple and effective way to avoid the above problems of vacuum insulation boards. The use of vacuum insulation boards in the form of internal insulation of the external wall has the advantages of convenient construction, greatly extended service life, relatively simple later maintenance, and less condensation and condensation at the board attachment position. However, there are currently few vacuum insulation boards on the market that are suitable for the construction of internal insulation of external walls.

[0005] Chinese patent CN116803679A discloses a vacuum insulation panel core material and preparation method and a vacuum insulation panel and preparation method. The vacuum insulation panel includes a core material, a protective layer and a barrier film; wherein the raw materials of the core material are 50-70 parts of glass fiber, 8-15 parts of fumed silica, 10-20 parts of straw powder, 2-7 parts of sunscreen, and 1-6 parts of getter; the protective layer is ultra-fine glass wool. The vacuum insulation panel obtained by this patent uses relatively expensive fumed silica as the core material, and the cost is relatively high. In addition, the panel surface is not effectively protected, and it is difficult to be used in the occasion of internal insulation of exterior walls, because the panel surface of the vacuum insulation panel is directly used as the interior wall surface of the room, which is difficult to resist collision and impact, and the insulation function is easily damaged.

[0006] Chinese patent CN116714342A discloses a metal sheet STP vacuum insulation sandwich insulation decorative panel process, including: S1, raw material selection and processing; S2, engraving and bending the metal plate; S3, core anchor installation; S4, STP vacuum insulation panel and metal plate composite; S5, backing perforated calcium silicate board composite; S6, sandwich anchor assembly installation. The present invention uses aluminum plate and calcium silicate board to connect the upper and lower sides of the STP vacuum insulation panel, so that the STP vacuum insulation core material is completely wrapped, avoiding damage to the STP vacuum insulation panel during processing, transportation, installation and later use. The patent insulation panel is protected by inorganic plates on both sides, one side is aluminum plate and the other side is calcium silicate plate, which will undoubtedly increase the overall weight of the panel and affect the convenience of construction. In addition, the aluminum plate has high thermal conductivity. Once the vacuum insulation panel is damaged, it will be attached to the aluminum plate, which will form a serious thermal bridge effect and greatly reduce the insulation performance of the vacuum insulation panel.

[0007] From the above, we can see that vacuum insulation panels still have problems such as relatively expensive core material costs, easy damage during construction, and not suitable for exterior wall insulation. Therefore, it is of great practical significance to develop vacuum internal insulation decorative panels that can be used for exterior wall insulation construction. Summary of the invention

[0008] In view of the deficiencies in the above-mentioned prior art, the present invention provides an integrated vacuum internal insulation decorative panel for existing buildings and a preparation method thereof, so as to achieve the following invention objectives: to prepare a vacuum internal insulation decorative panel with low core material cost, low thermal conductivity, resistance to water vapor transmission, not easy to damage the panel surface, convenient construction and suitable for internal insulation of exterior walls.

[0009] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0010] An integrated vacuum internal insulation decorative panel for existing buildings and a preparation method thereof, wherein the integrated vacuum internal insulation decorative panel for existing buildings is formed by bonding and compounding a decorative layer and an inner layer, wherein the decorative layer is a PVC integrated panel, the inner layer is a vacuum insulation panel, and the adhesive used for bonding the decorative layer and the inner layer is a room temperature curing two-component polyurethane adhesive;

[0011] The thickness of the PVC integrated board is 2-6 mm, and the thickness of the vacuum insulation board is 10-30 mm;

[0012] The vacuum insulation panel is composed of a composite core material, a bagged getter, and a barrier film bag;

[0013] The composite core material is composed of modified sepiolite, modified lignin powder and wood fiber;

[0014] The wood fiber has a diameter of 10-50 μm and a length of 500-2000 μm;

[0015] The barrier film bag adopts a 4-layer structure, which is composed of polyethylene film, aluminum foil, aluminized polyethylene terephthalate film, and nylon film from the innermost layer contacting the core material to the outside.

[0016] The thickness of the polyethylene film is 30-60 μm;

[0017] The thickness of the aluminum foil is 5-10 μm;

[0018] The thickness of the aluminized polyethylene terephthalate film is 7 to 15 μm;

[0019] The thickness of the nylon membrane is 12-20 μm;

[0020] The bagged getter is calcium oxide powder encapsulated in non-woven fabric, wherein the particle size of the calcium oxide powder is 3-10 μm;

[0021] The following are further improvements to the above technical solution:

[0022] Step 1, preparation of modified sepiolite

[0023] After the sepiolite is dried at 80-110°C for 15-24 hours, it is added to a dispersion kettle, and then chloroform and oleylamine are added. After the dispersion rate is controlled at 5000-9000 rpm and the dispersion is vigorously dispersed for 6-13 hours, the temperature is increased and kept constant at 50-80°C, the dispersion rate is reduced to 1500-3000 rpm, and the reaction system is kept under condensation reflux state, and docosanoic acid is added. After stirring for 15-30 minutes, thionyl chloride is added dropwise. After the addition is completed, the dispersion reaction is continued at a constant temperature for 4-7 hours, and then the reaction is stopped, the temperature is cooled to room temperature, and the filtered solid is washed with anhydrous ethanol for 3-5 times, and then dried at 60-95°C for 6-9 hours to obtain the modified sepiolite.

[0024] The average particle size of the sepiolite is 30-1000 nm;

[0025] The mass ratio of the sepiolite, chloroform, oleylamine, behenic acid and thionyl chloride is 15-35:100-150:1-4:3-9:0.1-0.5;

[0026] The thionyl chloride is added dropwise at a speed of 0.01-0.04 g / s.

[0027] Step 2: Preparation of modified lignin powder

[0028] After drying the lignin powder at 90-120° C. for 5-10 hours, the powder is placed in a ball mill, and then anhydrous ethanol and trichloromethylsilane are added, the speed of the ball mill is controlled to be 90-150 rpm, and the material temperature of the material in the ball mill is controlled to be 50-80° C. After ball milling until the average particle size of the lignin powder is 0.5-3 μm, the material is discharged, centrifuged, and the separated solid is washed with anhydrous ethanol for 3-5 times, and then placed in a 70-90° C. oven for drying for 7-12 hours to obtain a modified lignin powder;

[0029] The particle size of the lignin powder is 10-20 μm;

[0030] The mass ratio of the lignin powder, anhydrous ethanol and trichloromethylsilane is 20-40:60-120:4-8.

[0031] Step 3: Preparation of composite core material

[0032] After drying wood fiber, modified lignin powder and modified sepiolite at 90-120°C for 8-14 hours, the wood fiber, modified lignin powder and modified sepiolite are placed in a V-type powder mixer, and then the stirring rate is controlled at 150-400 rpm, and the mixture is stirred and mixed for 10-18 hours, and then the mixture is discharged to obtain a powder mixture, and then the powder mixture is placed in a non-woven bag, and after the bag opening is sewn, the non-woven bag filled with the powder mixture is placed in a molding machine, and the molding is performed under a controlled pressure of 3-15 MPa, and the outer non-woven bag is removed after the pressure is released to obtain a plate-shaped composite core material;

[0033] The mass ratio of the wood fiber, the modified lignin powder and the modified sepiolite is 50-80:15-35:15-30.

[0034] Step 4: Preparation of vacuum insulation panels

[0035] The composite core material is dried at 90-120°C for 3-6 hours, the barrier film bag is placed in a 40-50°C oven and dried for 110-150 minutes, and then the composite core material and the bagged getter are placed in a barrier film bag with three-side sealed edges. The barrier film bag containing the composite core material is then placed flat in a vacuum packaging machine and evacuated. The vacuum chamber of the vacuum packaging machine is evacuated to a high vacuum state of 0.1-0.3 Pa, and the pressure is maintained for 800-1300 seconds after the vacuum degree becomes constant. Then, the heat sealing electrode is turned on to heat-seal the bag opening. After the heat sealing is completed, the vacuum is removed to obtain a vacuum insulation panel.

[0036] Step 5: Preparation of vacuum internal insulation decorative panels

[0037] After spraying the room temperature curing two-component polyurethane glue on one side of the vacuum insulation board, the PVC integrated board is tightly attached to the glued board surface. After curing at room temperature for 24 to 30 hours, an integrated vacuum internal insulation decorative board for existing buildings is obtained.

[0038] Compared with the prior art, the present invention achieves the following beneficial effects:

[0039] 1. The present invention uses oleylamine as a surfactant, disperses sepiolite in chloroform, and then reacts with docosanoic acid under the catalysis of thionyl chloride, and the hydroxyl groups on the surface of the sepiolite react to obtain hydrophobic modification. The modified hydrophobic sepiolite can enhance the water vapor permeation resistance of the vacuum thermal insulation decorative board, and also enhances the mixing uniformity of the sepiolite and other powder materials;

[0040] 2. The present invention uses trichloromethylsilane to modify the surface of lignin powder, thereby enhancing the hydrophobicity of the lignin surface and making the lignin powder fluffy and easy to disperse. This not only increases the uniformity of the lignin powder when mixed with the modified sepiolite, but also ensures that the modified sepiolite can fill the gaps formed by the modified lignin powder during molding. In this way, the path of the trace air retained in the core material of the vacuum thermal insulation decorative board becomes tortuous and long, so that it is almost static, thereby obtaining the core material of the vacuum thermal insulation decorative board with very good thermal insulation performance;

[0041] 3. The present invention uses micron-grade lignin powder, sepiolite rich in nano-grade micropores and low-cost wood fiber to obtain a core material with good thermal insulation effect through a dry molding process. The cost of sepiolite is relatively low, so the cost of this core material is relatively low. Both lignin powder and wood fiber are renewable resources and are relatively environmentally friendly.

[0042] 4. The present invention attaches a PVC integrated board to one side of the vacuum insulation board. This design can effectively avoid collision and impact on the vacuum insulation board during the construction process, making the construction process quick and convenient. Secondly, the PVC integrated board can be directly used as an interior wall decoration surface. Therefore, the integrated vacuum internal insulation decorative board for existing buildings obtained by the present invention is very suitable for external wall insulation and is suitable for insulation decoration renovation of old existing buildings.

[0043] 5. The integrated vacuum internal insulation decorative board for existing buildings obtained by the present invention has a peel strength of 4.31~4.65N / 15mm, a heat sealing strength of 61.35~67.62N / 15mm, a wear resistance (mass loss) of 18.94~21.33mg, a maximum puncture resistance of 22.75~23.43N, a thermal conductivity of 3.73~4.02mW / (m·K), and a thermal conductivity of 3.94~4.11mW / (m·K) after 80 high temperature-water spraying cycles. DETAILED DESCRIPTION

[0044] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0045] Example 1: A method for preparing an integrated vacuum internal insulation decorative panel for existing buildings

[0046] Step 1, preparation of modified sepiolite

[0047] After the sepiolite is dried at 100°C for 19 hours, it is added to a dispersion kettle, and then chloroform and oleylamine are added. After the dispersion rate is controlled at 8000 rpm, the dispersion is vigorously dispersed for 11 hours, the temperature is increased and kept constant at 70°C, the dispersion rate is reduced to 2000 rpm, and the reaction system is kept in a condensation reflux state, and docosanoic acid is added. After stirring for 18 minutes, thionyl chloride is added dropwise. After the addition is completed, the dispersion reaction is continued at a constant temperature for 6 hours, the reaction is stopped, the temperature is cooled to room temperature, and the filtered solid is washed with anhydrous ethanol for 4 times, and then dried at 90°C for 8 hours to obtain modified sepiolite.

[0048] The average particle size of the sepiolite is 700 nm;

[0049] The mass ratio of the sepiolite, chloroform, oleylamine, behenic acid and thionyl chloride is 20:130:2:8:0.2;

[0050] The thionyl chloride is added dropwise at a speed of 0.03 g / s.

[0051] Step 2: Preparation of modified lignin powder

[0052] After drying the lignin powder at 100° C. for 9 hours, the powder was placed in a ball mill, and then anhydrous ethanol and trichloromethylsilane were added. The speed of the ball mill was controlled at 130 rpm, and the material temperature of the material in the ball mill was controlled at 70° C. After ball milling until the average particle size of the lignin powder was 2 μm, the material was discharged and centrifuged. The separated solid was washed with anhydrous ethanol for 4 times, and then dried in an oven at 85° C. for 10 hours to obtain a modified lignin powder.

[0053] The particle size of the lignin powder is 16 μm;

[0054] The mass ratio of the lignin powder, anhydrous ethanol and trichloromethylsilane is 35:90:7.

[0055] Step 3: Preparation of composite core material

[0056] After drying wood fiber, modified lignin powder and modified sepiolite at 100° C. for 11 hours, the wood fiber, modified lignin powder and modified sepiolite are placed in a V-type powder mixer, and then stirred and mixed for 16 hours at a stirring rate of 350 rpm, and then the materials are discharged to obtain a powder mixture, and then the powder mixture is placed in a non-woven bag, and after the bag opening is sewn, the non-woven bag filled with the powder mixture is placed in a molding machine, and the molding is performed under a controlled pressure of 10 MPa, and the outer non-woven bag is removed after the pressure is released to obtain a plate-shaped composite core material;

[0057] The wood fiber has a diameter of 40 μm and a length of 1200 μm;

[0058] The mass ratio of the wood fiber, the modified lignin powder and the modified sepiolite is 70:25:20.

[0059] Step 4: Preparation of vacuum insulation panels

[0060] The composite core material is dried at 110°C for 4 hours, and the barrier film bag is placed in a 47°C oven for 135 minutes. The composite core material and the bagged getter are then placed in a barrier film bag with three edges sealed. The barrier film bag containing the composite core material is then placed flat in a vacuum packaging machine and evacuated. The vacuum chamber of the vacuum packaging machine is evacuated to a high vacuum state of 0.2 Pa, and the pressure is maintained for 1000 seconds after the vacuum degree is constant. The heat sealing electrode is then turned on to heat seal the bag opening. After the heat sealing is completed, the vacuum is removed to obtain a vacuum insulation panel.

[0061] The barrier film bag adopts a 4-layer structure, which is composed of polyethylene film, aluminum foil, aluminized polyethylene terephthalate film, and nylon film from the innermost layer contacting the core material to the outside.

[0062] The thickness of the polyethylene film is 48 μm;

[0063] The thickness of the aluminum foil is 8 μm;

[0064] The thickness of the aluminized polyethylene terephthalate film is 10 μm;

[0065] The thickness of the nylon membrane is 17 μm;

[0066] The bagged getter is calcium oxide powder encapsulated in non-woven fabric, wherein the particle size of the calcium oxide powder is 8 μm.

[0067] Step 5: Preparation of vacuum internal insulation decorative panels

[0068] After spraying the room temperature curing two-component polyurethane glue on one side of the vacuum insulation board, the PVC integrated board is closely attached to the glued board surface, and after curing at room temperature for 29 hours, an integrated vacuum internal insulation decorative board for existing buildings is obtained;

[0069] The thickness of the PVC integrated board is 5 mm, and the thickness of the vacuum insulation board is 19 mm;

[0070] The specific brand of the room temperature curing two-component polyurethane adhesive is Henkel Loctite UK3131.

[0071] Example 2: A method for preparing an integrated vacuum internal insulation decorative panel for existing buildings

[0072] Step 1, preparation of modified sepiolite

[0073] After the sepiolite is dried at 80°C for 15 hours, it is added to a dispersion kettle, and then chloroform and oleylamine are added. After the dispersion rate is controlled at 5000 rpm, the dispersion is vigorously dispersed for 6 hours, the temperature is increased and kept constant at 50°C, the dispersion rate is reduced to 1500 rpm, and the reaction system is kept in a condensation reflux state, and docosanoic acid is added. After stirring for 15 minutes, thionyl chloride is added dropwise. After the addition is completed, the dispersion reaction is continued at a constant temperature for 4 hours, and then the reaction is stopped, the temperature is cooled to room temperature, and the filtered solid is washed with anhydrous ethanol for 3 times, and then dried at 60°C for 6 hours to obtain modified sepiolite.

[0074] The average particle size of the sepiolite is 30 nm;

[0075] The mass ratio of the sepiolite, chloroform, oleylamine, behenic acid and thionyl chloride is 15:100:1:3:0.1;

[0076] The thionyl chloride is added dropwise at a speed of 0.01 g / s.

[0077] Step 2: Preparation of modified lignin powder

[0078] After drying the lignin powder at 90° C. for 5 hours, the powder was placed in a ball mill, and then anhydrous ethanol and trichloromethylsilane were added. The speed of the ball mill was controlled to be 90 rpm, and the material temperature of the material in the ball mill was controlled to be 50° C. After ball milling until the average particle size of the lignin powder was 0.5 μm, the material was discharged and centrifuged. The separated solid was washed with anhydrous ethanol for 3 times, and then placed in a 70° C. oven for 7 hours to obtain a modified lignin powder.

[0079] The particle size of the lignin powder is 10 μm;

[0080] The mass ratio of the lignin powder, anhydrous ethanol and trichloromethylsilane is 20:60:4.

[0081] Step 3: Preparation of composite core material

[0082] After drying wood fiber, modified lignin powder and modified sepiolite at 90° C. for 8 hours, the wood fiber, modified lignin powder and modified sepiolite are placed in a V-type powder mixer, and then stirred and mixed for 10 hours at a stirring rate of 150 rpm, and then the materials are discharged to obtain a powder mixture, and then the powder mixture is placed in a non-woven bag, and after the bag opening is sewn, the non-woven bag filled with the powder mixture is placed in a molding machine, and the molding is performed under a controlled pressure of 3 MPa, and after the pressure is released, the outer non-woven bag is removed to obtain a plate-shaped composite core material;

[0083] The wood fiber has a diameter of 10 μm and a length of 500 μm;

[0084] The mass ratio of the wood fiber, the modified lignin powder and the modified sepiolite is 50:15:15.

[0085] Step 4: Preparation of vacuum insulation panels

[0086] The composite core material is dried at 90°C for 3 hours, and the barrier film bag is placed in a 40°C oven for drying for 110 minutes. The composite core material and the bagged getter are then placed in a barrier film bag with three edges sealed. The barrier film bag containing the composite core material is then placed flat in a vacuum packaging machine and evacuated. The vacuum chamber of the vacuum packaging machine is evacuated to a high vacuum state of 0.1 Pa, and the pressure is maintained for 800 seconds after the vacuum degree is constant. The heat sealing electrode is then turned on to heat seal the bag opening. After the heat sealing is completed, the vacuum is removed to obtain a vacuum insulation panel.

[0087] The barrier film bag adopts a 4-layer structure, which is composed of polyethylene film, aluminum foil, aluminized polyethylene terephthalate film, and nylon film from the innermost layer contacting the core material to the outside.

[0088] The thickness of the polyethylene film is 30 μm;

[0089] The thickness of the aluminum foil is 5 μm;

[0090] The thickness of the aluminized polyethylene terephthalate film is 7 μm;

[0091] The thickness of the nylon membrane is 12 μm;

[0092] The bagged getter is calcium oxide powder encapsulated in non-woven fabric, wherein the particle size of the calcium oxide powder is 3 μm.

[0093] Step 5: Preparation of vacuum internal insulation decorative panels

[0094] After spraying the room temperature curing two-component polyurethane glue on one side of the vacuum insulation board, the PVC integrated board is closely attached to the glued board surface, and after curing at room temperature for 24 hours, an integrated vacuum internal insulation decorative board for existing buildings is obtained;

[0095] The thickness of the PVC integrated board is 2 mm, and the thickness of the vacuum insulation board is 10 mm;

[0096] The specific brand of the room temperature curing two-component polyurethane adhesive is Henkel Loctite UK3131.

[0097] Example 3: A method for preparing an integrated vacuum internal insulation decorative panel for existing buildings

[0098] Step 1, preparation of modified sepiolite

[0099] After the sepiolite is dried at 110°C for 24 hours, it is added to a dispersion kettle, and then chloroform and oleylamine are added. The dispersion rate is controlled at 9000 rpm, and the dispersion is vigorously dispersed for 13 hours. The temperature is increased and kept constant at 80°C, and the dispersion rate is reduced to 3000 rpm. The reaction system is kept under condensation reflux state, and docosanoic acid is added. After stirring for 30 minutes, thionyl chloride is added dropwise. After the addition is completed, the dispersion reaction is continued at a constant temperature for 7 hours, and then the reaction is stopped, the temperature is cooled to room temperature, and the filtered solid is washed with anhydrous ethanol for 5 times, and then dried at 95°C for 9 hours to obtain modified sepiolite.

[0100] The average particle size of the sepiolite is 1000nm;

[0101] The mass ratio of the sepiolite, chloroform, oleylamine, behenic acid and thionyl chloride is 35:150:4:9:0.5;

[0102] The thionyl chloride is added dropwise at a speed of 0.04 g / s.

[0103] Step 2: Preparation of modified lignin powder

[0104] After drying the lignin powder at 120° C. for 10 hours, the powder was placed in a ball mill, and then anhydrous ethanol and trichloromethylsilane were added. The speed of the ball mill was controlled to be 150 rpm, and the temperature of the material in the ball mill was controlled to be 80° C. After ball milling until the average particle size of the lignin powder was 3 μm, the material was discharged and centrifuged. The separated solid was washed with anhydrous ethanol for 5 times, and then dried in an oven at 90° C. for 12 hours to obtain a modified lignin powder.

[0105] The particle size of the lignin powder is 20 μm;

[0106] The mass ratio of the lignin powder, anhydrous ethanol and trichloromethylsilane is 40:120:8.

[0107] Step 3: Preparation of composite core material

[0108] After drying wood fiber, modified lignin powder and modified sepiolite at 120° C. for 14 hours, the wood fiber, modified lignin powder and modified sepiolite are placed in a V-type powder mixer, and then stirred and mixed for 18 hours at a stirring rate of 400 rpm, and then the materials are discharged to obtain a powder mixture, and then the powder mixture is placed in a non-woven bag, and after the bag opening is sewn, the non-woven bag filled with the powder mixture is placed in a molding machine, and the molding is performed under a controlled pressure of 15 MPa, and the outer non-woven bag is removed after the pressure is released to obtain a plate-shaped composite core material;

[0109] The wood fiber has a diameter of 50 μm and a length of 2000 μm;

[0110] The mass ratio of the wood fiber, the modified lignin powder and the modified sepiolite is 80:35:30.

[0111] Step 4: Preparation of vacuum insulation panels

[0112] The composite core material is dried at 120°C for 6 hours, and the barrier film bag is placed in a 50°C oven for 150 minutes for drying. The composite core material and the bagged getter are then placed in a barrier film bag with three edges sealed. The barrier film bag containing the composite core material is then placed flat in a vacuum packaging machine and evacuated. The vacuum chamber of the vacuum packaging machine is evacuated to a high vacuum state of 0.3 Pa, and the pressure is maintained for 1300 seconds after the vacuum degree is constant. The heat sealing electrode is then turned on to heat seal the bag opening. After the heat sealing is completed, the vacuum is removed to obtain a vacuum insulation panel.

[0113] The barrier film bag adopts a 4-layer structure, which is composed of polyethylene film, aluminum foil, aluminized polyethylene terephthalate film, and nylon film from the innermost layer contacting the core material to the outside.

[0114] The thickness of the polyethylene film is 60 μm;

[0115] The thickness of the aluminum foil is 10 μm;

[0116] The thickness of the aluminized polyethylene terephthalate film is 15 μm;

[0117] The thickness of the nylon membrane is 20 μm;

[0118] The bagged getter is calcium oxide powder encapsulated in non-woven fabric, wherein the particle size of the calcium oxide powder is 10 μm.

[0119] Step 5: Preparation of vacuum internal insulation decorative panels

[0120] After spraying the room temperature curing two-component polyurethane adhesive on one side of the vacuum insulation board, the PVC integrated board is closely attached to the adhesive-coated board surface, and after curing at room temperature for 30 hours, an integrated vacuum internal insulation decorative board for existing buildings is obtained;

[0121] The thickness of the PVC integrated board is 6 mm, and the thickness of the vacuum insulation board is 30 mm;

[0122] The specific brand of the room temperature curing two-component polyurethane adhesive is Henkel Loctite UK3131.

[0123] Comparative Example 1: Based on Example 1, step 1, preparation of modified sepiolite and step 2, preparation of modified lignin powder were not performed. In step 3, 25 parts of modified lignin powder and 20 parts of modified sepiolite were replaced by 25 parts of lignin powder and 20 parts of sepiolite in equal amounts. The specific operation was as follows:

[0124] Do not perform steps 1 and 2;

[0125] Step 3: Preparation of composite core material

[0126] After drying wood fiber, lignin powder and sepiolite at 100° C. for 11 hours, the wood fiber, lignin powder and sepiolite are placed in a V-type powder mixer, and then stirred and mixed for 16 hours at a stirring rate of 350 rpm, and then the materials are discharged to obtain a powder mixture, and then the powder mixture is put into a non-woven bag, and after the bag opening is sewn, the non-woven bag filled with the powder mixture is placed in a molding machine, and the molding is performed under a controlled pressure of 10 MPa, and the outer non-woven bag is removed after the pressure is released to obtain a plate-shaped composite core material;

[0127] The wood fiber has a diameter of 40 μm and a length of 1200 μm;

[0128] The average particle size of the sepiolite is 700 nm;

[0129] The particle size of the lignin powder is 16 μm;

[0130] The mass ratio of the wood fiber, lignin powder and sepiolite is 70:25:20;

[0131] The operations of steps 4 and 5 are the same as those of Example 1.

[0132] Comparative Example 2: Based on Example 1, step 1, preparation of modified sepiolite, is not performed. In step 3, 20 parts of modified sepiolite are replaced by 20 parts of modified lignin powder. The specific operation is as follows:

[0133] Step 1, preparation of modified sepiolite is not performed

[0134] Step 2: The operation is the same as in Example 1;

[0135] Step 3: Preparation of composite core material

[0136] After drying wood fiber and modified lignin powder at 100° C. for 11 hours, the powder is placed in a V-type powder mixer, and then the stirring rate is controlled to be 350 rpm. After stirring and mixing for 16 hours, the material is discharged to obtain a powder mixture, and then the powder mixture is put into a non-woven bag. After the bag mouth is sewn, the non-woven bag filled with the powder mixture is placed in a molding machine, and the molding is performed under a controlled pressure of 10 MPa. After the pressure is released, the outer non-woven bag is removed to obtain a plate-shaped composite core material;

[0137] The wood fiber has a diameter of 40 μm and a length of 1200 μm;

[0138] The mass ratio of the wood fiber to the modified lignin powder is 70:45;

[0139] The operations of steps 4 and 5 are the same as those of Example 1.

[0140] Comparative Example 3: Based on Example 1, step 2, preparation of modified lignin powder, is not performed. In step 3, 25 parts of modified lignin powder are replaced by 25 parts of modified sepiolite in equal amounts. The specific operation is as follows:

[0141] The operation of step 1 is the same as that of embodiment 1;

[0142] Step 2, preparation of modified lignin powder, is not performed;

[0143] Step 3: Preparation of composite core material

[0144] After drying wood fiber and modified sepiolite at 100°C for 11 hours, the wood fiber and modified sepiolite are placed in a V-type powder mixer, and then stirred and mixed for 16 hours at a stirring rate of 350 rpm, and then discharged to obtain a powder mixture, and then the powder mixture is put into a non-woven bag, and after the bag opening is sewn, the non-woven bag filled with the powder mixture is placed in a molding machine, and the molding is performed under a controlled pressure of 10 MPa, and the outer non-woven bag is removed after the pressure is released to obtain a plate-shaped composite core material;

[0145] The wood fiber has a diameter of 40 μm and a length of 1200 μm;

[0146] The mass ratio of the wood fiber to the modified sepiolite is 70:45;

[0147] The operations of steps 4 and 5 are the same as those of Example 1.

[0148] Performance Test:

[0149] The following performance indicators were tested for the integrated vacuum internal insulation decorative panels for existing buildings obtained in Examples 1, 2, 3 and Comparative Examples 1, 2, 3:

[0150] 1. Test the peel strength according to GB / T 8808-1998 Peel Test Method Standard for Soft Composite Plastic Materials;

[0151] 2. Test the heat seal strength according to "QB / T 2358-1998 Test method for heat seal strength of plastic packaging";

[0152] 3. Test the wear resistance with reference to GB / T1768-1979 Determination of Weathering Resistance of Paint Film;

[0153] 4. Refer to GB / T 37608-2019 Vacuum Insulation Panel to test the maximum puncture resistance of the non-PVC board surface of the above decorative board (i.e. the side not bonded with the PVC integrated board);

[0154] 5. Test the thermal conductivity in accordance with GB / T 39704-2020 Determination of effective thermal conductivity of vacuum insulation panels;

[0155] 6. Refer to the high temperature-water spraying cycle test in "JG / T 287-2013 Insulation Decorative Panel External Wall External Insulation System Materials" to test the thermal conductivity of the decorative panel after 80 high temperature-water spraying cycles. The specific conditions of the high temperature-water spraying cycle are: each cycle lasts 6 hours, the surface of the sample is heated to 70℃ and maintained at 70±5℃ for 3 hours, and then the surface is sprayed with water for 1 hour, the water temperature is 15±5℃, and the water volume is 1L / (m 2 ·min), and then let it stand for 2 hours;

[0156] The specific test results are shown in Table 1:

[0157] Table 1

[0158]

[0159] From the data in Table 1, it can be seen that the thermal conductivity coefficients of the three embodiments are very small, and the highest embodiment is only 4.02mW / (m·K), which shows that the integrated vacuum internal insulation decorative board for existing buildings prepared by the present invention has very excellent thermal insulation performance, and the integrated vacuum internal insulation decorative board for existing buildings obtained by the three embodiments has a negligible increase in thermal conductivity after 80 high-temperature-water spraying cycles, which shows that the vacuum insulation decorative board obtained by the present application has a good water vapor barrier effect, and the water absorption rate of the internal core material is also very low, so that the thermal insulation performance can be maintained without attenuation after 80 high-temperature water spraying cycles. The peel strength, heat sealing strength, wear resistance, maximum puncture resistance and The thermal conductivity of Example 1 is almost the same as that of Example 1, but the thermal conductivity of Examples 1, 2, and 3 is significantly higher than that of Example 1, which shows that the change of the core material has basically no effect on the mechanical properties of the decorative board membrane material, but has a significant effect on the thermal conductivity; in Example 1, the modified lignin powder and the modified sepiolite are all replaced by lignin powder and sepiolite, and the thermal conductivity of Example 1 is 2.47mW / (m·K) higher than that of Example 1, and the thermal conductivity of Example 1 increases by about 3mW / (m·K) after the high temperature-water spraying cycle. This may be due to the fact that the lignin powder is not surface modified, the fluffiness is relatively poor, the agglomeration is relatively serious, and the gaps between the powders are small, so that during the mixing and molding process, it is difficult to achieve a relatively uniform lignin powder and sepiolite powder. The uniform mixing degree makes it difficult to fill the pores formed by the lignin powder with the sepiolite powder, which results in an excessively large porosity inside the core material, a large degree of freedom of movement of the residual air, and a correspondingly poor insulation effect. In addition, the lignin powder and the sepiolite powder are not surface modified, and the water absorption is very strong, which may be the main reason why the thermal conductivity of the comparative example 1 increases by about 3mW / (m·K) after the high temperature-water spraying cycle; only modified lignin powder is added to the core material of the comparative example 2, and no modified sepiolite is added. The thermal conductivity of the comparative example 2 increases to 19.72mW / (m·K), which may be due to the fact that the particle size of the modified lignin powder does not reach the nanometer level, and at the same time, there is a lack of filling of the powder material such as sepiolite with rich nanometer-level internal pores, so the molding The size of the internal gap of the core material formed after the high temperature-water spraying cycle is too large, which leads to a very large thermal conductivity and a significant decrease in the thermal insulation effect. In addition, the thermal conductivity of Example 2 only increases by 1.23mW / (m·K) after the high temperature-water spraying cycle. This may be due to the reduced water absorption rate of the lignin powder after modification, which in turn reduces the water vapor absorption rate of the vacuum thermal insulation decorative board. The core material of Example 3 only adds modified sepiolite without modified lignin, and its thermal conductivity is also significantly higher than that of Example 1. This shows that it is difficult to obtain the best thermal insulation effect by only adding modified sepiolite, a powder material rich in nano-scale internal micropores. The combination of micron-scale modified lignin powder can improve the thermal insulation performance of the core material. The thermal conductivity of Example 3 increases by 1.49mW / (m·K), the increase is not large, which shows that modified sepiolite can also reduce the water absorption rate of the core material inside the vacuum thermal insulation decorative board.

[0160] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing an integrated vacuum internal insulation decorative panel for existing buildings, characterized in that: The preparation method of the integrated vacuum internal insulation decorative board for existing buildings comprises five steps: preparation of modified sepiolite, preparation of modified lignin powder, preparation of composite core material, preparation of vacuum insulation board, and preparation of vacuum internal insulation decorative board; The preparation method of the modified sepiolite is as follows: after drying the sepiolite at 80-110°C for 15-24 hours, the sepiolite is added to a dispersion kettle, chloroform and oleylamine are added, and the dispersion rate is controlled at 5000-9000 rpm. After strong dispersion for 6-13 hours, the temperature is increased and kept constant at 50-80°C, the dispersion rate is reduced to 1500-3000 rpm, and the reaction system is kept in a condensation reflux state, and docosanoic acid is added. After stirring for 15-30 minutes, thionyl chloride is added dropwise. After the addition is completed, the dispersion reaction is continued at a constant temperature for 4-7 hours, the reaction is stopped, the temperature is cooled to room temperature, and the filtered solid is washed with anhydrous ethanol for 3-5 times, and then dried at 60-95°C for 6-9 hours to obtain the modified sepiolite. The average particle size of the sepiolite is 30-1000 nm; The preparation method of the modified lignin powder is as follows: after drying the lignin powder at 90-120° C. for 5-10 hours, putting the powder into a ball mill, then adding anhydrous ethanol and trichloromethylsilane, controlling the speed of the ball mill to 90-150 rpm, controlling the material temperature of the material in the ball mill to 50-80° C., ball milling until the average particle size of the lignin powder is 0.5-3 μm, discharging the material, centrifuging, washing the separated solid with anhydrous ethanol for 3-5 times, and drying it in an oven at 70-90° C. for 7-12 hours to obtain the modified lignin powder; The particle size of the lignin powder is 10-20 μm; The composite core material is prepared by: drying wood fiber, modified lignin powder and modified sepiolite at 90-120°C for 8-14 hours, placing them in a V-shaped powder mixer, and then stirring and mixing them at a stirring rate of 150-400 rpm for 10-18 hours, discharging the materials to obtain a powder mixture, and then putting the powder mixture into a non-woven bag, sewing the bag mouth, placing the non-woven bag filled with the powder mixture into a molding machine, controlling the pressure at 3-15 MPa for molding, and removing the outer non-woven bag after pressure relief to obtain a plate-shaped composite core material; The preparation method of the vacuum insulation panel is as follows: drying the composite core material at 90-120°C for 3-6 hours, placing the barrier film bag in a 40-50°C oven for drying for 110-150 minutes, then placing the composite core material and the bagged getter in a barrier film bag with three edges sealed, then placing the barrier film bag containing the composite core material flat in a vacuum packaging machine, evacuating the vacuum chamber of the vacuum packaging machine to a high vacuum state of 0.1-0.3 Pa, and maintaining the pressure for 800-1300 seconds after the vacuum degree is constant, then opening the heat sealing electrode to heat-seal the bag opening, and removing the vacuum after the heat sealing is completed to obtain the vacuum insulation panel; The preparation method of the vacuum internal insulation decorative board is as follows: after spraying room temperature curing two-component polyurethane glue on one side of the vacuum insulation board, the PVC integrated board is tightly attached to the glued board surface, and after curing at room temperature for 24 to 30 hours, the integrated vacuum internal insulation decorative board for existing buildings is obtained.

2. The method for preparing the integrated vacuum internal insulation decorative panel for existing buildings according to claim 1, characterized in that: The mass ratio of the sepiolite, chloroform, oleylamine, behenic acid and thionyl chloride is 15-35:100-150:1-4:3-9:0.1-0.5; The thionyl chloride is added dropwise at a speed of 0.01-0.04 g / s.

3. The method for preparing the integrated vacuum internal insulation decorative panel for existing buildings according to claim 1, characterized in that: The mass ratio of the lignin powder, anhydrous ethanol and trichloromethylsilane is 20-40:60-120:4-8.

4. The method for preparing the integrated vacuum internal insulation decorative panel for existing buildings according to claim 1 is characterized in that: The wood fiber has a diameter of 10-50 μm and a length of 500-2000 μm; The mass ratio of the wood fiber, the modified lignin powder and the modified sepiolite is 50-80:15-35:15-30.

5. The method for preparing the integrated vacuum internal insulation decorative panel for existing buildings according to claim 1, characterized in that: The barrier film bag adopts a 4-layer structure, which is composed of polyethylene film, aluminum foil, aluminized polyethylene terephthalate film, and nylon film from the innermost layer contacting the core material to the outside. The thickness of the polyethylene film is 30-60 μm; The thickness of the aluminum foil is 5-10 μm; The thickness of the aluminized polyethylene terephthalate film is 7 to 15 μm; The thickness of the nylon membrane is 12-20 μm; The bagged getter is calcium oxide powder encapsulated in non-woven fabric, wherein the particle size of the calcium oxide powder is 3-10 μm.

6. The method for preparing the integrated vacuum internal insulation decorative panel for existing buildings according to claim 1, characterized in that: The thickness of the PVC integrated board is 2-6 mm, and the thickness of the vacuum insulation board is 10-30 mm.

7. The integrated vacuum internal insulation decorative board for existing buildings obtained by the preparation method according to any one of claims 1 to 6 is characterized in that: The integrated vacuum internal insulation decorative panel for existing buildings is composited by bonding a decorative layer and an inner layer, wherein the decorative layer is a PVC integrated panel, the inner layer is a vacuum insulation panel, and the glue used for bonding the decorative layer and the inner layer is a two-component polyurethane glue that cures at room temperature.

Citation Information

Patent Citations

  • Metal thin plate STP vacuum heat insulation sandwich heat preservation decoration plate technology

    CN116714342A

  • Vacuum insulated panel core material and preparation method thereof, vacuum insulated panel and preparation method thereof

    CN116803679A

  • Environment-friendly water tank and production process thereof

    CN106433400A

  • Plastic masterbatch and preparation method thereof

    CN111534002A

  • Environment-friendly flame-retardant insulating material and preparation method thereof