A large-particle, low-temperature stable styrene-butadiene latex and preparation method thereof
By controlling the reaction conditions and the combination of additives of styrene butadiene latex, the problem of poor stability of large-particle styrene butadiene latex in low-temperature environments is solved, and the particle size increase and mechanical performance improvement is achieved, which is suitable for bonding applications in low-temperature environments.
Patent Information
- Application Number
- CN202411146776.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing large-particle styrene butadiene latex has poor stability and mechanical properties in low-temperature environments and is difficult to maintain effectively.
The reaction temperature and stirring conditions were controlled by the mixing and concentration method of styrene butadiene latex emulsion under two different conditions, and the average particle size was formed of 320 by combining deionized water, nitrogen replacement, initiator, emulsifier and pH regulator. -420nm large-particle styrene butadiene latex, and a stabilizer, defoaming agent, chelating agent and agglomerating agent are added to improve its stability and mechanical properties.
It achieves good stability and mechanical properties of styrene butadiene latex in low temperature environments, and is resistant to low temperatures to -57℃, which is suitable for use as an auxiliary material for adhesives.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of styrene butadiene latex, and in particular relates to a large-particle, low-temperature stable styrene butadiene latex and a preparation method thereof. Background Art
[0002] Large particle size SBR latex is a type of SBR latex with larger particle size. It is usually used in specific applications, such as adhesives, coatings and repair materials, where larger particle size is required to provide better coverage and adhesion. Its preparation method is similar to that of ordinary SBR latex, which is a stable emulsion formed by low temperature polymerization of butadiene and styrene.
[0003] At present, there are several ways to synthesize large-particle styrene butadiene latex. One is to control the emulsification concentration, reaction temperature, stirring speed and other conditions to allow the latex particles to directly polymerize to form large-particle styrene butadiene latex. The other is to first prepare small-particle styrene butadiene latex, and then polymerize the small-particle styrene butadiene latex to form large-particle styrene butadiene latex through post-treatment such as cooling temperature, pH value adjustment, concentration and filtration.
[0004] For example, the Chinese patent with application number "CN202211553981.3" discloses "a method for preparing large-particle-size and wide-distribution styrene-butadiene latex", and its content is: "In the present invention, cationic emulsifiers and pH regulators are added during the polymerization process to agglomerate the latex particles. Due to the strong electrostatic attraction between anions and cations, more latex particles will be adsorbed around the cationic emulsifier. As the reaction proceeds, the volume of the latex particles continues to increase, and these particles collide with each other and agglomerate into large particles. At the same time, the compound of anionic and cationic emulsifiers will produce a strong electrical effect, which can reduce the effectiveness of surface tension, reduce the CMC of the system, increase the polymerization site, and achieve a wide distribution of particle size. Large-particle-size and wide-distribution styrene-butadiene latex is a high-functional synthetic latex. Because of its large particle size and wide distribution, it remains fluid at high solid content and is widely used in papermaking, carpets, foam rubber, asphalt modification, ABS and other production fields."
[0005] Another example is the Chinese patent with application number "CN202311165456.9", which discloses "a method for preparing large-particle-size high-solid-content styrene-butadiene latex", and its content is: "A method for preparing large-particle-size high-solid-content styrene-butadiene latex, N-(4-bromophenyl) maleimide and di(p-aminophenoxy) dimethylsilane undergo substitution reaction to obtain bisphenyl maleimide siloxane. Then, it is copolymerized with montmorillonite under the initiation of dibenzoyl peroxide to obtain polybis(2-phenyl) maleimide siloxane. Phenylmaleimidesiloxane grafted montmorillonite. Styrene, divinylbenzene and butadiene undergo polymerization reaction under the initiation of potassium persulfate to obtain large-particle styrene butadiene latex, to which sodium oleate is added to obtain large-particle styrene butadiene latex with high solid content. Finally, polybiphenylmaleimidesiloxane grafted montmorillonite and styrene butadiene latex are stirred evenly, sliced, vulcanized and hot-pressed to obtain high-temperature resistant styrene butadiene rubber. The styrene butadiene rubber prepared by the present invention has excellent high-temperature resistance and mechanical properties.
[0006] The large-particle styrene-butadiene latex produced by the above-mentioned preparation methods all have good high-temperature resistance, but when faced with a low-temperature environment, its stability and mechanical properties are difficult to maintain effectively. Summary of the invention
[0007] In view of the above defects, the purpose of the present invention is to provide a large-particle, low-temperature stable styrene butadiene latex and a preparation method thereof, aiming to solve the problem of poor stability and mechanical properties of large-particle styrene butadiene latex in a low-temperature environment in the prior art.
[0008] In order to solve the above technical problems, the technical solution of the present invention is:
[0009] A method for preparing a large-particle-size, low-temperature-stable styrene-butadiene latex comprises the following steps: step 1, feeding deionized water into a reactor, and then feeding nitrogen into the reactor to replace the air in the reactor, after the replacement is completed, mixing styrene, a first initiator, a first emulsifier and a pH regulator with the deionized water and stirring, feeding a mixed gas of nitrogen and butadiene into the reactor during the stirring process, during which the temperature in the reactor rises to 50-70°C, the pH value is 6-8, and after the reaction is completed, a first primary styrene-butadiene latex with an average particle size of 60-80 nm is obtained;
[0010] Step 2, deionized water is introduced into the reactor, and then nitrogen is introduced into the reactor to replace the air in the reactor. After the replacement is completed, styrene, a second initiator, a second emulsifier, an antifreeze agent and a pH regulator are mixed with the deionized water and stirred. During the stirring process, a mixed gas of nitrogen and butadiene is introduced into the reactor. During this process, the temperature in the reactor is adjusted to 5-10° C. and the pH value is 6-8. After the reaction is completed, a second primary styrene-butadiene rubber latex with an average particle size of 50-70 nm is obtained;
[0011] Step 3, mixing the first primary styrene butadiene latex solution in step 1 with the second primary styrene butadiene latex solution in step 2 at a volume ratio of 2.5-3:7-7.5 to obtain a secondary styrene butadiene latex solution;
[0012] Step 4, stirring and mixing the secondary styrene butadiene latex solution, stabilizer, defoamer, chelating agent and agglomerating agent at a stirring speed of 120-150 r / min and a stirring temperature of 20-30° C. After stirring, sending the mixed solution to a vacuum kettle, adjusting the temperature in the vacuum kettle to 70-90° C., and concentrating for 3-5 hours to obtain large-particle styrene butadiene latex;
[0013] In step 1 and step 2, the volume ratio of butadiene to nitrogen in the mixed gas is 2:1.
[0014] Wherein, in step 1, by weight, styrene is 40-45 parts, butadiene is 30-35 parts, the first initiator is 4-6 parts, the first emulsifier is 10-12 parts, and the pH adjuster is 1-3 parts.
[0015] Wherein, in step 1, the first initiator is composed of a mixture of potassium persulfate and sodium sulfite, with 50-60 parts of potassium persulfate and 40-50 parts of sodium sulfite by weight.
[0016] Wherein, in step 1, the first emulsifier is composed of a mixture of alkyl sulfonate, fatty acid soap and polyoxyethylene alcohol; in terms of weight, the alkyl sulfonate is 20-30 parts, the fatty acid soap is 20-30 parts, and the polyoxyethylene alcohol is 40-60 parts.
[0017] Wherein, in step 2, by weight, styrene is 40-45 parts, butadiene is 28-32 parts, the second initiator is 4-6 parts, the second emulsifier is 8-10 parts, the pH adjuster is 1-3 parts, and the antifreeze agent is 4-7 parts.
[0018] Wherein, in step 2, the second initiator is composed of ammonium persulfate and hydrogen peroxide; by weight, the ammonium persulfate is 60-70 parts, and the hydrogen peroxide is 30-40 parts.
[0019] Wherein, in step 2, the second emulsifier is composed of a mixture of dodecyltrimethylammonium bromide, benzyltrimethylammonium chloride and octadecyltrimethylammonium bromide; by weight, 30-40 parts of dodecyltrimethylammonium bromide, 20-30 parts of benzyltrimethylammonium chloride and 30-40 parts of octadecyltrimethylammonium bromide.
[0020] The antifreeze agent is composed of one or more of ethylene glycol, propylene glycol, glycerol, ethanol and isopropanol.
[0021] Wherein, in step 4, by weight, the secondary styrene-butadiene latex solution is 75-80 parts, the stabilizer is 4-6 parts, the defoamer is 2-4 parts, the chelating agent is 3-5 parts, and the agglomerating agent is 5-10 parts; the stabilizer is composed of a mixture of bisphenol A and carboxymethyl cellulose, by weight, bisphenol A is 30-40 parts, and carboxymethyl cellulose is 60-70 parts; the defoamer is silicone oil; the chelating agent is EDTA or DTPA; and the agglomerating agent is tetrabutyl titanate.
[0022] Among them, the average particle size of styrene butadiene latex is 320-420nm.
[0023] After adopting the above technical solution, the beneficial effects of this solution are:
[0024] First, the particle size of the finished product of styrene butadiene latex is relatively large, with an average particle size between 320-420nm. Second, styrene butadiene latex has good low temperature resistance and good stability in low temperature environments, and its low temperature resistance is around -57°C. Third, styrene butadiene latex has good mechanical properties and viscosity, which makes it suitable for use as an auxiliary material for adhesives in low temperature environments. DETAILED DESCRIPTION
[0025] Example:
[0026] A large-particle, low-temperature stable styrene-butadiene latex and a preparation method thereof, comprising the following steps:
[0027] Step 1: Deionized water is introduced into the reactor, and then nitrogen is introduced into the reactor to replace the air in the reactor. After the replacement is completed, styrene, a first initiator, a first emulsifier and a pH regulator are mixed with deionized water and stirred. During the stirring process, a mixed gas of nitrogen and butadiene is introduced into the reactor. During this process, the temperature in the reactor rises to 50-70° C., and the pH value is 6-8. After the reaction is completed, a first primary styrene-butadiene latex with an average particle size of 60-80 nm is obtained. The first primary styrene-butadiene latex mainly has good stability and monomer concentration.
[0028] Step 2: Deionized water is introduced into the reactor, and then nitrogen is introduced into the reactor to replace the air in the reactor. After the replacement is completed, styrene, a second initiator, a second emulsifier, an antifreeze agent and a pH regulator are mixed with deionized water and stirred. During the stirring process, a mixed gas of nitrogen and butadiene is introduced into the reactor. During this process, the temperature in the reactor is adjusted to 5-10° C., and the pH value is 6-8. After the reaction is completed, a second primary styrene-butadiene latex with an average particle size of 50-70 nm is obtained. The second primary styrene-butadiene latex has good low-temperature stability and mechanical properties.
[0029] Step 3, mixing the first primary styrene butadiene latex solution in step 1 with the second primary styrene butadiene latex solution in step 2 at a volume ratio of 2.5-3:7-7.5 to obtain a secondary styrene butadiene latex solution;
[0030] Step 4: Stir and mix the secondary styrene butadiene latex solution, stabilizer, defoamer, chelating agent and agglomerating agent at a stirring speed of 120-150 r / min and a stirring temperature of 20-30°C. After stirring, send the mixed solution to a vacuum autoclave, adjust the temperature in the vacuum autoclave to 70-90°C, and concentrate for 3-5 hours to obtain large-particle styrene butadiene latex.
[0031] This scheme prepares different styrene butadiene latex emulsions through two preparation methods, so that the two different styrene butadiene latex solutions have different physical properties, and then the two are mixed and concentrated and purified to increase the particle size of the styrene butadiene latex and obtain a large-particle-size styrene butadiene latex solution.
[0032] The average particle size of the finished styrene butadiene latex is 320-420nm.
[0033] In step 1, by weight, 40-45 parts of styrene, 30-35 parts of butadiene, 4-6 parts of the first initiator, 10-12 parts of the first emulsifier, and 1-3 parts of the pH adjuster are used.
[0034] In step 1, the first initiator is composed of a mixture of potassium persulfate and sodium sulfite, with 50-60 parts of potassium persulfate and 40-50 parts of sodium sulfite by weight. Potassium persulfate and sodium sulfite are used in combination to form a red oxygen initiation system at a higher temperature, thereby effectively guiding particle polymerization to form a styrene-butadiene latex with a larger particle size.
[0035] In step 1, the first emulsifier is composed of alkyl sulfonate, fatty acid soap and polyoxyethylene alcohol; by weight, 20-30 parts of alkyl sulfonate, 20-30 parts of fatty acid soap and 40-60 parts of polyoxyethylene alcohol. The first emulsifier is a composite emulsifier composed of an anionic emulsifier and a nonionic emulsifier. The first primary styrene-butadiene latex has a good emulsifying effect and has a relatively long-lasting stability.
[0036] In step 1 and step 2, the volume ratio of butadiene to nitrogen in the mixed gas is 2:1.
[0037] In step 2, by weight, 40-45 parts of styrene, 28-32 parts of butadiene, 4-6 parts of the second initiator, 8-10 parts of the second emulsifier, 1-3 parts of the pH regulator, and 4-7 parts of the antifreeze agent are used.
[0038] In step 2, the second initiator is composed of ammonium persulfate and hydrogen peroxide; by weight, the ammonium persulfate is 60-70 parts and the hydrogen peroxide is 30-40 parts. The use of ammonium persulfate and hydrogen peroxide together allows the second primary styrene butadiene latex to polymerize at a relatively low temperature, thereby ensuring the mechanical properties and stability of the second primary styrene butadiene latex in a low temperature environment.
[0039] In step 2, the second emulsifier is composed of a mixture of dodecyl trimethyl ammonium bromide, benzyl trimethyl ammonium chloride, and octadecyl trimethyl ammonium bromide; by weight, 30-40 parts of dodecyl trimethyl ammonium bromide, 20-30 parts of benzyl trimethyl ammonium chloride, and 30-40 parts of octadecyl trimethyl ammonium bromide. The second emulsifier is composed of a cationic emulsifier, which makes the styrene-butadiene latex solution have good dispersibility, and the particles are easier to aggregate to form large-size particles.
[0040] The antifreeze is composed of one or more of ethylene glycol, propylene glycol, glycerol, ethanol and isopropanol.
[0041] In step 4, by weight, the secondary styrene-butadiene latex solution is 75-80 parts, the stabilizer is 4-6 parts, the defoamer is 2-4 parts, the chelating agent is 3-5 parts, and the agglomerating agent is 5-10 parts; the stabilizer is composed of a mixture of bisphenol A and carboxymethyl cellulose, by weight, bisphenol A is 30-40 parts, and carboxymethyl cellulose is 60-70 parts; the defoamer is silicone oil; the chelating agent is EDTA or DTPA; and the agglomerating agent is tetrabutyl titanate.
[0042] Stabilizers can effectively inhibit polymer degradation caused by oxidation. Chelating agents react with metal particles introduced during the preparation of styrene-butadiene latex to form stable complexes, blocking their catalytic activity, thereby ensuring that the polymer can be stable in both low and high temperature environments. The role of agglomerating agents is to improve the mechanical strength and weather resistance of the finished product.
[0043] In this embodiment, the pH adjuster is sodium hydroxide, potassium hydroxide, sodium carbonate, or the pH adjuster is one of acetic acid, citric acid, and dilute hydrochloric acid.
[0044] The pH adjuster needs to be selected according to the pH value in the reactor. When the pH value is low, the pH adjuster is sodium hydroxide, potassium hydroxide, or sodium carbonate. When the pH value is too high, the pH adjuster is one of acetic acid, citric acid, or dilute hydrochloric acid.
[0045] Embodiment 1:
[0046] According to the above preparation method, styrene-butadiene latex is prepared, wherein in step 1, by weight, styrene is 40 parts, butadiene is 30 parts, the first initiator is 4 parts, the first emulsifier is 10 parts, and the pH adjuster is 1 part. The temperature in the reactor rises to 50° C. and the pH value is 6.
[0047] The first initiator is composed of 50 parts of potassium persulfate and 50 parts of sodium sulfite.
[0048] The first emulsifier consists of 20 parts of alkyl sulfonate, 20 parts of fatty acid soap and 60 parts of polyoxyethylene alcohol.
[0049] In step 2, by weight, 40 parts of styrene, 28 parts of butadiene, 4 parts of the second initiator, 8 parts of the second emulsifier, 1 part of the pH regulator, and 4 parts of the antifreeze agent are used. The temperature in the reactor is adjusted to 5° C. and the pH value is 6.
[0050] The second initiator consists of 60 parts of ammonium persulfate and 40 parts of hydrogen peroxide.
[0051] The second emulsifier is composed of 30 parts of dodecyltrimethylammonium bromide, 30 parts of benzyltrimethylammonium chloride, and 40 parts of octadecyltrimethylammonium bromide.
[0052] The antifreeze is ethylene glycol.
[0053] In step three, the first primary styrene butadiene latex solution and the second primary styrene butadiene latex solution are mixed in a volume ratio of 2.5:7.5.
[0054] In step 4, by weight, 75 parts of secondary styrene-butadiene latex solution, 4 parts of stabilizer, 2 parts of defoamer, 3 parts of chelating agent, and 5 parts of agglomerating agent are used; the stirring speed is 120 r / min, the stirring temperature is 20°C, the temperature in the vacuum autoclave is adjusted to 70°C, and the concentration time is 3h.
[0055] The stabilizer is composed of 30 parts of bisphenol A and 70 parts of carboxymethyl cellulose; the chelating agent is EDTA.
[0056] Embodiment 2:
[0057] According to the above preparation method, styrene-butadiene latex is prepared, wherein in step 1, by weight, styrene is 42 parts, butadiene is 31 parts, the first initiator is 5 parts, the first emulsifier is 11 parts, and the pH adjuster is 2 parts. The temperature in the reactor rises to 60° C. and the pH value is 7.
[0058] The first initiator is composed of 55 parts of potassium persulfate and 45 parts of sodium sulfite.
[0059] The first emulsifier is composed of 25 parts of alkyl sulfonate, 25 parts of fatty acid soap and 50 parts of polyoxyethylene alcohol.
[0060] In step 2, by weight, 42 parts of styrene, 30 parts of butadiene, 5 parts of the second initiator, 9 parts of the second emulsifier, 2 parts of the pH regulator, and 5 parts of the antifreeze agent are used. The temperature in the reactor is adjusted to 6° C. and the pH value is 7.
[0061] The second initiator consists of 65 parts of ammonium persulfate and 35 parts of hydrogen peroxide.
[0062] The second emulsifier is composed of 32 parts of dodecyltrimethylammonium bromide, 29 parts of benzyltrimethylammonium chloride, and 39 parts of octadecyltrimethylammonium bromide.
[0063] Antifreeze is a mixture of ethylene glycol and glycerin.
[0064] In step three, the first primary styrene butadiene latex solution and the second primary styrene butadiene latex solution are mixed in a volume ratio of 2.7:7.3.
[0065] In step 4, by weight, there are 76 parts of secondary styrene-butadiene latex solution, 5 parts of stabilizer, 3 parts of defoamer, 4 parts of chelating agent, and 6 parts of agglomerating agent; the stirring speed is 130 r / min, the stirring temperature is 25°C, the temperature in the vacuum autoclave is adjusted to 75°C, and the concentration time is 4h.
[0066] The stabilizer is composed of 35 parts of bisphenol A and 65 parts of carboxymethyl cellulose; the chelating agent is DTPA.
[0067] Embodiment 3:
[0068] According to the above preparation method, styrene-butadiene latex was prepared, wherein in step 1, by weight, styrene was 43 parts, butadiene was 34 parts, the first initiator was 5.5 parts, the first emulsifier was 11.5 parts, and the pH adjuster was 2.5 parts. The temperature in the reactor was raised to 65° C., and the pH value was 7.5.
[0069] The first initiator is composed of 56 parts of potassium persulfate and 44 parts of sodium sulfite.
[0070] The first emulsifier is composed of 28 parts of alkyl sulfonate, 28 parts of fatty acid soap and 44 parts of polyoxyethylene alcohol.
[0071] In step 2, by weight, 44 parts of styrene, 31 parts of butadiene, 5.5 parts of the second initiator, 9.5 parts of the second emulsifier, 2.5 parts of the pH adjuster, and 6 parts of the antifreeze agent are used. The temperature in the reactor is adjusted to 7° C. and the pH value is 7.5.
[0072] The second initiator consists of 68 parts of ammonium persulfate and 32 parts of hydrogen peroxide.
[0073] The second emulsifier is composed of 35 parts of dodecyltrimethylammonium bromide, 22 parts of benzyltrimethylammonium chloride, and 38 parts of octadecyltrimethylammonium bromide.
[0074] Antifreeze is a mixture of ethanol and isopropyl alcohol.
[0075] In step three, the first primary styrene butadiene latex solution and the second primary styrene butadiene latex solution are mixed in a volume ratio of 2.8:7.2.
[0076] In step 4, by weight, 77 parts of secondary styrene-butadiene latex solution, 5.5 parts of stabilizer, 3.5 parts of defoamer, 4.5 parts of chelating agent, and 7 parts of agglomerating agent are used; the stirring speed is 140 r / min, the stirring temperature is 26°C, the temperature in the vacuum kettle is adjusted to 80°C, and the concentration time is 4.5 hours.
[0077] The stabilizer is composed of 37 parts of bisphenol A and 63 parts of carboxymethyl cellulose; the chelating agent is DTPA.
[0078] Embodiment 4:
[0079] According to the above preparation method, styrene-butadiene latex is prepared, wherein in step 1, by weight, styrene is 45 parts, butadiene is 35 parts, the first initiator is 6 parts, the first emulsifier is 12 parts, and the pH adjuster is 3 parts. The temperature in the reactor rises to 70° C. and the pH value is 8.
[0080] The first initiator is composed of 60 parts of potassium persulfate and 40 parts of sodium sulfite.
[0081] The first emulsifier consists of 30 parts of alkyl sulfonate, 30 parts of fatty acid soap and 40 parts of polyoxyethylene alcohol.
[0082] In step 2, by weight, 45 parts of styrene, 32 parts of butadiene, 6 parts of the second initiator, 10 parts of the second emulsifier, 3 parts of the pH adjuster, and 7 parts of the antifreeze agent are used. The temperature in the reactor is adjusted to 10° C. and the pH value is 8.
[0083] The second initiator consists of 70 parts of ammonium persulfate and 30 parts of hydrogen peroxide.
[0084] The second emulsifier is composed of 40 parts of dodecyltrimethylammonium bromide, 20 parts of benzyltrimethylammonium chloride, and 40 parts of octadecyltrimethylammonium bromide.
[0085] Antifreeze is a mixture of ethylene glycol, propylene glycol, glycerin, ethanol and isopropyl alcohol.
[0086] In step three, the first primary styrene butadiene latex solution and the second primary styrene butadiene latex solution are mixed in a volume ratio of 3:7.
[0087] In step 4, by weight, 80 parts of secondary styrene-butadiene latex solution, 6 parts of stabilizer, 4 parts of defoamer, 5 parts of chelating agent, and 10 parts of agglomerating agent are used; the stirring speed is 150 r / min, the stirring temperature is 30°C, the temperature in the vacuum autoclave is adjusted to 90°C, and the concentration time is 5 hours.
[0088] The stabilizer is composed of 40 parts of bisphenol A and 60 parts of carboxymethyl cellulose; the chelating agent is EDTA.
[0089] Comparative Example 1:
[0090] This comparative example is different from Example 1 in that the first initiator is not used.
[0091] Comparative Example 2:
[0092] This comparative example is different from Example 1 in that the first emulsifier is not used.
[0093] Comparative Example 3:
[0094] The difference between this comparative example and Example 1 is that no second initiator is used.
[0095] Comparative Example 4:
[0096] This comparative example is different from Example 1 in that no second emulsifier is used.
[0097] Comparative Example 5:
[0098] The difference between this comparative example and Example 1 is that no antifreeze agent is used.
[0099] Comparative Example 6:
[0100] This comparative example is different from Example 1 in that no stabilizer is used.
[0101] Comparative Example 7:
[0102] The difference between this comparative example and Example 1 is that no chelating agent is used.
[0103] Comparative Example 8:
[0104] This comparative example differs from Example 1 in that no agglomerating agent is used.
[0105] Comparative Example 9:
[0106] The difference between this comparative example and Example 1 is that the volume ratio of the first primary styrene butadiene latex to the second primary styrene butadiene latex is 5:5.
[0107] The styrene-butadiene latex products in Examples 1-4 and Comparative Examples 1-9 were tested respectively, and the test results are as follows:
[0108]
[0109] As can be seen from the table above, this solution has the following advantages: First, the particle size of the finished product of styrene butadiene latex is relatively large, with an average particle size between 320-420nm. Second, styrene butadiene latex has good low temperature resistance and good stability in low temperature environments, and its low temperature resistance is around -57°C. Third, styrene butadiene latex has good mechanical properties and viscosity, which enables it to be used as an auxiliary material for adhesives in low temperature environments.
[0110] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.
Claims
1. A method for preparing a large-particle, low-temperature stable styrene-butadiene latex, characterized in that: The method comprises the following steps: step 1, introducing deionized water into a reactor, and then introducing nitrogen into the reactor to replace the air in the reactor, and after the replacement, mixing styrene, a first initiator, a first emulsifier and a pH regulator with the deionized water and stirring, and introducing a mixed gas of nitrogen and butadiene into the reactor during the stirring process, during which the temperature in the reactor rises to 50-70° C., and the pH value is 6-8, and after the reaction is completed, a first primary styrene-butadiene rubber latex with an average particle size of 60-80 nm is obtained; Step 2, deionized water is introduced into the reactor, and then nitrogen is introduced into the reactor to replace the air in the reactor. After the replacement is completed, styrene, a second initiator, a second emulsifier, an antifreeze agent and a pH regulator are mixed with the deionized water and stirred. During the stirring process, a mixed gas of nitrogen and butadiene is introduced into the reactor. During this process, the temperature in the reactor is adjusted to 5-10° C. and the pH value is 6-8. After the reaction is completed, a second primary styrene-butadiene rubber latex with an average particle size of 50-70 nm is obtained; Step 3, mixing the first primary styrene butadiene latex solution in step 1 with the second primary styrene butadiene latex solution in step 2 at a volume ratio of 2.5-3:7-7.5 to obtain a secondary styrene butadiene latex solution; Step 4, stirring and mixing the secondary styrene butadiene latex solution, stabilizer, defoamer, chelating agent and agglomerating agent at a stirring speed of 120-150 r / min and a stirring temperature of 20-30° C. After stirring, sending the mixed solution to a vacuum kettle, adjusting the temperature in the vacuum kettle to 70-90° C., and concentrating for 3-5 hours to obtain large-particle styrene butadiene latex; In step 1 and step 2, the volume ratio of butadiene to nitrogen in the mixed gas is 2:1; In step 1, by weight, 40-45 parts of styrene, 30-35 parts of butadiene, 4-6 parts of the first initiator, 10-12 parts of the first emulsifier, and 1-3 parts of the pH adjuster; In step 1, the first initiator is composed of a mixture of potassium persulfate and sodium sulfite, with 50-60 parts of potassium persulfate and 40-50 parts of sodium sulfite by weight; In step 1, the first emulsifier is composed of a mixture of alkyl sulfonate, fatty acid soap and polyoxyethylene alcohol; by weight, the alkyl sulfonate is 20-30 parts, the fatty acid soap is 20-30 parts, and the polyoxyethylene alcohol is 40-60 parts; In step 2, by weight, 40-45 parts of styrene, 28-32 parts of butadiene, 4-6 parts of the second initiator, 8-10 parts of the second emulsifier, 1-3 parts of the pH adjuster, and 4-7 parts of the antifreeze agent; In step 2, the second initiator is composed of ammonium persulfate and hydrogen peroxide; by weight, the ammonium persulfate is 60-70 parts and the hydrogen peroxide is 30-40 parts; In step 2, the second emulsifier is composed of a mixture of dodecyltrimethylammonium bromide, benzyltrimethylammonium chloride, and octadecyltrimethylammonium bromide; by weight, 30-40 parts of dodecyltrimethylammonium bromide, 20-30 parts of benzyltrimethylammonium chloride, and 30-40 parts of octadecyltrimethylammonium bromide; In step 4, by weight, the secondary styrene-butadiene latex solution is 75-80 parts, the stabilizer is 4-6 parts, the defoamer is 2-4 parts, the chelating agent is 3-5 parts, and the agglomerating agent is 5-10 parts; the stabilizer is composed of a mixture of bisphenol A and carboxymethyl cellulose, by weight, bisphenol A is 30-40 parts, and carboxymethyl cellulose is 60-70 parts; the defoamer is silicone oil; the chelating agent is EDTA or DTPA; and the agglomerating agent is tetrabutyl titanate.
2. The method for preparing a large-particle, low-temperature stable styrene-butadiene latex according to claim 1, characterized in that: The antifreeze is composed of one or more of ethylene glycol, propylene glycol, glycerol, ethanol and isopropanol.