A glass fiber organic glass reinforced PVC composite plate and preparation method thereof
By introducing glass fiber plexiglass into PVC composite sheets, and through specific process flows and raw material ratios, the problem of low strength and tensile properties of PVC composite sheets has been solved, and its strength and anti-aging properties have been significantly improved to meet the needs of high-end customers. performance application requirements.
Patent Information
- Application Number
- CN202411172742.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Existing PVC composite panels have low strength and tensile properties, making it difficult to meet the needs of certain high-performance applications.
The preparation method of glass fiber plexiglass reinforced PVC composite sheets is adopted. By evenly heating the reactor and mixing it with the prepolymer, the curing process and the hot pressing process are carried out to form a composite material of glass fiber plexiglass and PVC to improve its strength and Tensile capacity, and through specific raw material ratio and process optimization, the mechanical properties and aging resistance of the material are enhanced.
It significantly improves the strength, anti-aging performance and service life of PVC composite panels, solves the problem of dispersion and compatibility of glass fiber during processing, and enhances the overall structural stability and mechanical properties of the material.
Abstract
Description
Technical Field
[0001] The invention relates to the field of PVC composite sheets, and in particular to a glass fiber organic glass reinforced PVC composite sheet and a preparation method thereof. Background Art
[0002] In the automotive, construction, energy, industrial and transportation industries, material solutions are gradually changing. The shift from traditional materials to high-performance composites provides market opportunities for the rapid promotion and use of high-performance composites. Materials science, especially composites, is one of the main driving forces for technological development today. The increasing market demand for glass fiber and its composites has promoted the development of the glass fiber and its composites industry.
[0003] PVC is the world's most produced general-purpose plastic with a wide range of applications. There are two types of PVC: hard and soft. Hard polyvinyl chloride is used for building pipes, doors and windows. It is also used to make plastic bottles, packaging, bank cards or membership cards. Stabilizers, lubricants and fillers are added to PVC. After mixing, it can be extruded into hard pipes, special-shaped pipes, and corrugated pipes of various calibers using an extruder, which are used as sewer pipes, drinking water pipes, wire casings or stair handrails.
[0004] Patent publication number CN118344684A discloses a high-strength PVC composite board and its production process, which makes the composite board have good mechanical properties and impact strength by compounding glass fiber and PVC resin.
[0005] The patent with publication number CN118240129B discloses a high-transmittance acrylic resin and a high-transmittance photovoltaic front panel, and obtains a high-transmittance acrylic resin by hot-pressing and compounding nano-materials with glass fiber cloth.
[0006] It can be seen that material compounding is one of the common methods to improve material properties, but the strength and tensile properties of existing PVC composite boards are still relatively low. Summary of the invention
[0007] The object of the present invention is to provide a glass fiber organic glass reinforced PVC composite plate and a preparation method thereof, so as to solve the problem that the existing PVC composite plate has poor strength and tensile properties.
[0008] The embodiments of the present invention are implemented by the following technical solutions:
[0009] A method for preparing a glass fiber organic glass reinforced PVC composite plate, comprising:
[0010] S100, adding 400-500 parts of methyl methacrylate and 4-5 parts of initiator in a reaction kettle, uniformly heating to 80-100°C for 3.5-4.5 hours, then keeping the temperature constant for 1.5-2.5 hours, and finally cooling to below 30 degrees with frozen brine to obtain a prepolymer;
[0011] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0012] S300, compounding the glass fiber organic glass and the PVC material through a hot pressing process to obtain a glass fiber organic glass reinforced PVC composite plate.
[0013] The prepolymer can be made into particles with a particle size of 0.3-0.6mm.
[0014] After 1.5-2.5h of constant temperature reaction, the viscosity of the system reaches 5Pa·s. In order to ensure the cleanliness of the glass fiber surface and improve its adhesion with the prepolymer, the glass fiber can be cleaned, surface modified or coated before mixing with the prepolymer.
[0015] The curing process can adopt a physical thermosetting method, where the glass fiber is impregnated in the organic glass prepolymer and then cured at 70-80°C to form a sheet of suitable thickness, which can be selected to be 0.2-0.4mm.
[0016] S300 can also use a bonding process, but the environmental protection of bonding is poor, so the present invention uses a hot pressing process, first extrude the PVC powder through an extruder, put the glass fiber organic glass on the top and bottom of the extruded PVC, stack the two together, and then press the two together through a hot press. The hot pressing temperature can be selected from 120-160°C, the pressure can be selected from 55-70Pa, and the hot pressing speed can be selected from 3-5 meters / minute.
[0017] The composite material obtained by compounding glass fiber and prepolymer with PVC greatly enhances the strength of PVC and prolongs its service life. PVC is between two layers of glass fiber organic glass. The PVC layer can increase the thickness of the board and avoid the cost problem caused by the board being made entirely of glass fiber organic glass. When the PVC composite board is pressed, the glass fiber can improve the tensile strength of the organic glass layer.
[0018] Preferably, in parts by weight, the curing process comprises: adding 120-180 parts of glass fiber, 300-450 parts of prepolymer, 70-100 parts of maleic acid, 1.5-3 parts of emulsifier and 2-4 parts of initiator to 600-800 parts of methyl methacrylate, reacting at a temperature of 65-105°C for 5-10h to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 12-16 microns and the length is 0.25mm-0.5mm.
[0019] The compatibility of glass fiber and PMMA is poor, and the structural stability of glass fiber plexiglass obtained directly by thermosetting composite glass fiber and PMMA is poor. Especially in the process of subsequent processing and molding, the loosening of glass fiber in the system will affect the overall performance of the product, such as compressive strength and flexural strength. In order to improve the compatibility of glass fiber and PMMA, the applicant has made further improvements to the curing process, adopted a chemical curing process, and improved the structure of glass fiber plexiglass through the curing process to improve its strength, water resistance, heat resistance and acid and alkali resistance. By adding methyl methacrylate again and changing the ratio of the initiator twice, the amount of initiator used in the prepolymer preparation process is higher, the strength of the prepolymer is larger, and the amount of initiator used in the curing process is lower, making the glass fiber plexiglass easier to be evenly dispersed in the system and optimizing the product structure. The reaction system is a ternary copolymerization system, which makes the glass fiber plexiglass have the characteristics of high molecular weight and low cross-linking degree of PMMA, low molecular weight and high cross-linking degree of PMMA, and the characteristics after polymerization of MMA and maleic acid, so that the position stability of the glass fiber is enhanced during the molding process of the material, and the occurrence of floating fiber phenomenon is reduced. If all PMMA is high cross-linked, it is easy to age during use, and the deformation after aging will affect the compatibility of glass fiber and PMMA, further reducing the performance of the product after aging. If all PMMA is low cross-linked, its mechanical strength is insufficient. The present invention realizes that glass fiber organic glass is not easy to age, has stronger mechanical properties, and more uniform dispersion of glass fiber through reasonable curing process and raw material ratio. Even if the structure of the high cross-linked part ages, the overall deformation caused by aging is reduced under structural interlocking and structural compounding, and the stability of the overall structure of the material is increased. Maleic acid can also promote the uniform dispersion of glass fiber.
[0020] Preferably, in parts by weight, the addition operation of maleic acid in the curing process includes: adding 10-15 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 10-25 parts of maleic acid at a uniform speed within 2-4 hours, then adding 40-65 parts of maleic acid at a uniform speed within 1-2 hours, and finally adding 10-20 parts of maleic acid at a uniform speed within 3-4 hours.
[0021] If maleic acid is added to the reaction system at one time, the viscosity of the reaction system is difficult to control and increases rapidly, which is unfavorable for the uniform dispersion of glass fiber. The addition of maleic acid can increase the dispersibility of the system, but after reaching a certain amount, the dispersibility will decrease again. The one-time addition amount of maleic acid in the present invention is less, which can ensure the uniformity of the system, and the product structure with low cross-linking degree is more compatible with glass fiber. The addition speed of maleic acid increases during the secondary addition, which can make the raw materials polymerize quickly after the glass fiber is evenly dispersed and stable, improve the molecular weight and cross-linking degree of the material, and improve the mechanical properties of the product. The addition speed of maleic acid is reduced again during the three additions to avoid the reaction temperature from being continuously increased due to the excessively long time of the secondary addition, and heat is difficult to release in time. If the release problem of heat is solved by reducing the speed of the secondary addition, the orientation interaction of the rigid segment and the flexible segment in its segment structure is reduced, and then the phase separation strength of the two is reduced, and the complementary effect of the overall material is reduced, such as after the material is aged, the compensation of the low cross-linked structure to the deformation of the high cross-linked structure will be reduced. Since maleic acid also has the function of promoting the dispersion of glass fibers, a certain amount of maleic acid is added to the reaction system at one time in the present invention so as to uniformly disperse the glass fibers in the system. Since maleic acid will be continuously consumed during the reaction, the subsequent addition speed of maleic acid needs to meet the dispersion of the glass fibers while meeting the reaction rate requirements, thereby selecting a specific addition speed.
[0022] Parts by weight are calculated based on the total amount of maleic acid. For example, if the total amount of maleic acid is 500g, 10 parts are added once, 40 parts are added twice, and 10 parts are added three times, then 500*10 / (10+40+10)≈83.33g is added once.
[0023] Preferably, in parts by weight, the addition operation of the initiator in the curing process includes: firstly adding 0.5-1 parts of the initiator at a uniform speed within 2-4 hours, and then adding 1.5-3 parts of the initiator at a uniform speed within 1-2 hours.
[0024] The first addition of initiator can be synchronized with the first addition of maleic acid, and the second addition of initiator can also be synchronized with the second addition of maleic acid. The amount represented by one portion of initiator is consistent with the amount represented by one portion of prepolymer in the curing process.
[0025] The initial addition of initiator is relatively slow, the polymerization monomers have more time to be oriented, the polymerization product has higher crystallinity, and the heat resistance and strength of the material can be greatly improved. During the secondary addition, rapid polymerization between monomers is required, so the initiator addition speed is increased. At the same time, after the viscosity of the system increases, the initiator diffuses slowly, so the amount of initiator needs to be increased. Adding excess initiator during the secondary addition of maleic acid allows the initiator to be used for the reaction of the system when maleic acid is added three times, avoiding the contradiction of needing to reduce the reaction speed while the system viscosity is large and needing to increase the amount of initiator.
[0026] Preferably, the initiator includes one or more of azobisisobutyronitrile, benzoyl peroxide and a BPO / DMA mixed system, and the emulsifier includes one or more of OP-10, alkyl sulfate, polyoxyethylene ether and lecithin.
[0027] Through experiments, it was found that the product performance was best when the initiator was a BPO / DMA mixed system and the weight ratio of BPO to DMA was 0.65:1 when used once and 0.74:1 when used twice. OP-10 was the best emulsifier.
[0028] Preferably, in parts by weight, the glass fiber is pretreated before being mixed with the prepolymer, and the pretreatment operation includes: mixing 40-60 parts of maleic acid with 0.5-1.5 parts of silane coupling agent to obtain a mixed solution with a Ph value of 4-6, reacting the mixed solution at 50-60°C for 1-2.5h, adding 80-100 parts of glass fiber and 1-2 parts of catalyst, and immersing at 60-70°C for 5-8h to obtain the pretreated glass fiber.
[0029] Maleic acid can promote the hydrolysis of silane coupling agent. By controlling the amount of substances and the order of material addition, multiple reactions can be present in the system. For example, the glass fiber reacts with maleic acid under the action of a catalyst to increase the surface roughness of the glass fiber and the bonding degree between the glass fiber and the matrix material. The silane coupling agent reacts with maleic acid and then with the glass fiber to improve the interfacial adhesion. The silane coupling agent reacts with the glass fiber to form a chemical bond between the glass fiber and the matrix, thereby improving the bonding degree between the two.
[0030] Preferably, the catalyst comprises one or more of thionyl chloride, tetrabutyl titanate and benzenesulfonic acid.
[0031] Through experiments, it was found that tetrabutyl titanate is the best.
[0032] Preferably, the silane coupling agent includes one or more of KA1003, KBM-1003, KBM-403 and X-12-817H.
[0033] Through experiments, it was found that KBM-403 is the best.
[0034] Preferably, calcium-based grease is used to form a lubricating layer on the surface of the pretreated glass fiber, and the hydrolysis temperature of the lubricating layer is 60-80°C.
[0035] Calcium-based grease can increase the dispersibility of glass fibers in the initial stage of the curing process. After the glass fibers are dispersed, the lubricating layer hydrolyzes into water and carbon dioxide at the reaction temperature, exposing the pretreated surface of the glass fibers and increasing the bonding between the glass fibers and the matrix material.
[0036] A glass fiber organic glass reinforced PVC composite plate prepared by the preparation method.
[0037] The present invention has at least the following beneficial effects:
[0038] The PVC composite board provided by the present invention has the advantages of high strength, anti-aging and long service life; the present invention solves the problem of poor dispersibility of glass fiber during processing and the problem of poor compatibility between glass fiber and PMMA through an improved curing process; the pretreatment of the glass fiber further increases its bonding with the matrix material, and the lubricating layer further increases the dispersibility of the glass fiber. DETAILED DESCRIPTION
[0039] In order to make the purpose, method scheme and advantages of the embodiments of the present invention clearer, the method scheme in the embodiments of the present invention is clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0040] Embodiment 1: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0041] S100, after adding 400 parts of methyl methacrylate and 4 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 80°C over 3.5 hours, and then kept constant for 1.5 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA was 0.65:1 in parts by weight;
[0042] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0043] The curing process includes: adding 120 parts of glass fiber, 300 parts of prepolymer, 70 parts of maleic acid, 1.5 parts of OP-10 and 2 parts of BPO / DMA mixed system into 600 parts of methyl methacrylate at one time, with BPO:DMA=0.74:1 by weight, reacting at a temperature of 65°C for 5 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 12 microns and the length is 0.25 mm.
[0044] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0045] Embodiment 2: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0046] S100, after adding 500 parts of methyl methacrylate and 5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 80-100°C for 4.5 hours, and then kept constant for 2.5 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which BPO:DMA=0.65:1 in parts by weight;
[0047] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0048] The curing process includes: adding 180 parts of glass fiber, 450 parts of prepolymer, 100 parts of maleic acid, 3 parts of OP-10 and 4 parts of BPO / DMA mixed system into 800 parts of methyl methacrylate at one time, with BPO:DMA=0.74:1 by weight, reacting at a temperature of 105°C for 5-10 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 12-16 microns and the length is 0.5 mm.
[0049] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0050] Embodiment 3: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0051] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0052] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0053] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system into 700 parts of methyl methacrylate at one time, with BPO:DMA=0.74:1 by weight, reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0054] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0055] Embodiment 4: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0056] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0057] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0058] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0059] The adding operation of maleic acid in the curing process includes: adding 10 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 10 parts of maleic acid at a uniform speed within 2 hours, then adding 40 parts of maleic acid at a uniform speed within 1 hour, and finally adding 10 parts of maleic acid at a uniform speed within 3 hours.
[0060] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0061] Example 5: In parts by weight, a method for preparing a glass fiber organic glass reinforced PVC composite sheet comprises:
[0062] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0063] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0064] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0065] The addition operation of maleic acid in the curing process includes: adding 15 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 25 parts of maleic acid at a uniform speed within 4 hours, then adding 65 parts of maleic acid at a uniform speed within 2 hours, and finally adding 20 parts of maleic acid at a uniform speed within 4 hours.
[0066] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0067] Example 6: In parts by weight, a method for preparing a glass fiber organic glass reinforced PVC composite sheet comprises:
[0068] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0069] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0070] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0071] The addition operation of maleic acid in the curing process includes: adding 12 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 17 parts of maleic acid at a uniform speed within 3 hours, then adding 57 parts of maleic acid at a uniform speed within 1.5 hours, and finally adding 15 parts of maleic acid at a uniform speed within 3.5 hours.
[0072] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0073] Example 7: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0074] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0075] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0076] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0077] The addition operation of maleic acid in the curing process includes: adding 12 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 17 parts of maleic acid at a uniform speed within 3 hours, then adding 57 parts of maleic acid at a uniform speed within 1.5 hours, and finally adding 15 parts of maleic acid at a uniform speed within 3.5 hours.
[0078] The operation of adding the initiator in the curing process includes: firstly adding 0.5 parts of the initiator at a uniform speed within 2 hours, and then adding 1.5 parts of the initiator at a uniform speed within 1 hour.
[0079] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0080] Embodiment 8: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0081] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0082] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0083] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0084] The addition operation of maleic acid in the curing process includes: adding 12 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 17 parts of maleic acid at a uniform speed within 3 hours, then adding 57 parts of maleic acid at a uniform speed within 1.5 hours, and finally adding 15 parts of maleic acid at a uniform speed within 3.5 hours.
[0085] The operation of adding the initiator in the curing process includes: firstly adding 1 part of the initiator at a uniform speed within 4 hours, and then adding 3 parts of the initiator at a uniform speed within 2 hours.
[0086] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0087] Example 9: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0088] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0089] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0090] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0091] The addition operation of maleic acid in the curing process includes: adding 12 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 17 parts of maleic acid at a uniform speed within 3 hours, then adding 57 parts of maleic acid at a uniform speed within 1.5 hours, and finally adding 15 parts of maleic acid at a uniform speed within 3.5 hours.
[0092] The operation of adding the initiator in the curing process includes: firstly adding 0.75 parts of the initiator at a uniform speed within 3 hours, and then adding 2 parts of the initiator at a uniform speed within 1.5 hours.
[0093] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0094] Embodiment 10: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0095] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0096] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0097] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0098] The addition operation of maleic acid in the curing process includes: adding 12 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 17 parts of maleic acid at a uniform speed within 3 hours, then adding 57 parts of maleic acid at a uniform speed within 1.5 hours, and finally adding 15 parts of maleic acid at a uniform speed within 3.5 hours.
[0099] The operation of adding the initiator in the curing process includes: firstly adding 0.75 parts of the initiator at a uniform speed within 3 hours, and then adding 2 parts of the initiator at a uniform speed within 1.5 hours.
[0100] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0101] Before mixing with the prepolymer, the glass fiber is pretreated, and the pretreatment operation includes: mixing 40 parts of maleic acid with 0.5 parts of silane coupling agent to obtain a mixed solution with a Ph value of 4, reacting the mixed solution at 50°C for 1 hour, adding 80 parts of glass fiber and 1 part of catalyst, and immersing at 60°C for 5 hours to obtain the pretreated glass fiber.
[0102] Embodiment 11: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0103] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0104] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0105] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0106] The addition operation of maleic acid in the curing process includes: adding 12 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 17 parts of maleic acid at a uniform speed within 3 hours, then adding 57 parts of maleic acid at a uniform speed within 1.5 hours, and finally adding 15 parts of maleic acid at a uniform speed within 3.5 hours.
[0107] The operation of adding the initiator in the curing process includes: firstly adding 0.75 parts of the initiator at a uniform speed within 3 hours, and then adding 2 parts of the initiator at a uniform speed within 1.5 hours.
[0108] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0109] Before mixing with the prepolymer, the glass fiber is pretreated, and the pretreatment operation includes: mixing 60 parts of maleic acid with 1.5 parts of silane coupling agent to obtain a mixed solution with a Ph value of 6, reacting the mixed solution at 60°C for 2.5 hours, adding 100 parts of glass fiber and 2 parts of catalyst, and immersing at 70°C for 8 hours to obtain the pretreated glass fiber.
[0110] Example 12: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0111] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0112] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0113] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0114] The addition operation of maleic acid in the curing process includes: adding 12 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 17 parts of maleic acid at a uniform speed within 3 hours, then adding 57 parts of maleic acid at a uniform speed within 1.5 hours, and finally adding 15 parts of maleic acid at a uniform speed within 3.5 hours.
[0115] The operation of adding the initiator in the curing process includes: firstly adding 0.75 parts of the initiator at a uniform speed within 3 hours, and then adding 2 parts of the initiator at a uniform speed within 1.5 hours.
[0116] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0117] Before mixing with the prepolymer, the glass fiber is pretreated, and the pretreatment operation includes: mixing 50 parts of maleic acid with 1 part of silane coupling agent to obtain a mixed solution with a Ph value of 5, reacting the mixed solution at 55°C for 1.75 hours, adding 90 parts of glass fiber and 1.5 parts of catalyst, and immersing at 65°C for 6.5 hours to obtain the pretreated glass fiber.
[0118] Example 13: A method for preparing a glass fiber organic glass reinforced PVC composite sheet, in parts by weight, comprising:
[0119] S100, after adding 450 parts of methyl methacrylate and 4.5 parts of BPO / DMA mixed system into the reactor, the temperature was uniformly raised to 90°C for 4 hours, and then kept at a constant temperature for 2 hours, and finally cooled to below 30 degrees with frozen brine to obtain a prepolymer, in which the ratio of BPO:DMA is 0.65:1 in parts by weight;
[0120] S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass;
[0121] The curing process includes: adding 150 parts of glass fiber, 375 parts of prepolymer, 85 parts of maleic acid, 2 parts of OP-10 and 3 parts of BPO / DMA mixed system to 700 parts of methyl methacrylate, in which BPO:DMA=0.74:1 by weight, and reacting at a temperature of 80°C for 7 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 14 microns and the length is 0.4 mm.
[0122] The addition operation of maleic acid in the curing process includes: adding 12 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 17 parts of maleic acid at a uniform speed within 3 hours, then adding 57 parts of maleic acid at a uniform speed within 1.5 hours, and finally adding 15 parts of maleic acid at a uniform speed within 3.5 hours.
[0123] The operation of adding the initiator in the curing process includes: firstly adding 0.75 parts of the initiator at a uniform speed within 3 hours, and then adding 2 parts of the initiator at a uniform speed within 1.5 hours.
[0124] S300, compounding glass fiber organic glass and PVC material through hot pressing process to obtain glass fiber organic glass reinforced PVC composite sheet. First, PVC powder is extruded through an extruder, and the glass fiber organic glass is placed on the extruded PVC so that the two are stacked together, and then the two are pressed into shape through a hot press. The hot pressing temperature is 120°C, the pressure is 60Pa, and the hot pressing speed is 4 meters / minute.
[0125] Before mixing with the prepolymer, the glass fiber is pretreated, and the pretreatment operation includes: mixing 50 parts of maleic acid with 1 part of silane coupling agent to obtain a mixed solution with a Ph value of 5, reacting the mixed solution at 55° C. for 1.75 hours, adding 90 parts of glass fiber and 1.5 parts of catalyst, and immersing at 65° C. for 6.5 hours to obtain the pretreated glass fiber. A lubricating layer is formed on the surface of the pretreated glass fiber using calcium-based grease.
[0126] Experiment: The performance of the PVC composite sheet prepared by the preparation method of Examples 1-13 was tested. Each preparation method was repeated five times, and the performance test results were the average performance of the five products. In each of Examples 10-12, the catalyst of each example was selected from thionyl chloride, tetrabutyl titanate and benzenesulfonic acid, and 5 experiments were conducted respectively. The silane coupling agent was selected from KA1003, KBM-1003, KBM-403 and X-12-817H, and 5 experiments were conducted respectively. In Example 13, the catalyst was selected from tetrabutyl titanate, and the silane coupling agent was selected from KBM-403.
[0127] Performance test method: Hail impact resistance test: Take PVC products with different production times to make samples, use a steel ball drop tester to adjust a 1KG steel ball at a height of 1M, let it fall freely, hit the sample, and observe whether there is any damage. The test results are shown in Table 1 and Table 2.
[0128] Table 1
[0129] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Embodiment 13 Whether to destroy no no no no no no no no no no
[0130] Table 2
[0131] Thionyl chloride Tetrabutyl titanate Benzenesulfonic acid KA1003 no no no KBM-1003 no no no KBM-403 no no no X-12-817H no no no
[0132] It can be seen from Table 1 and Table 2 that the PVC composite sheet prepared by the preparation method of the present invention has good hail impact resistance.
[0133] Tensile strength and tensile elongation at break test: 5 specimens with specifications of 50×250×4 mm were made from composite PVC material, and tested using an MX-1080 tensile testing machine at a tensile speed of 50 mm / min to obtain tensile strength and elongation at break. The test results are shown in Tables 3, 4 and 5. Table 4 is the tensile strength test results of the PVC composite sheets prepared by the methods of Examples 10-12. Table 5 is the elongation at break test results of the PVC composite sheets prepared by the methods of Examples 10-12.
[0134] Table 3
[0135] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Embodiment 13 Tensile strength / MPa 85 98 103 117 122 125 137 145 147 186 Elongation at break / % 71 97 114 133 147 155 176 199 208 325
[0136] Table 4
[0137] Thionyl chloride Tetrabutyl titanate Benzenesulfonic acid KA1003 153MPa 162MPa 157MPa KBM-1003 150MPa 173MPa 160MPa KBM-403 174MPa 181MPa 168MPa X-12-817H 159MPa 171MPa 165MPa
[0138] Table 5
[0139] Thionyl chloride Tetrabutyl titanate Benzenesulfonic acid KA1003 278% 265% 243% KBM-1003 259% 284% 278% KBM-403 281% 307% 273% X-12-817H 268% 275% 263%
[0140] Impact strength test: 5 specimens were made from composite PVC products and tested on a simply supported beam double V-notch impact machine in accordance with the provisions of GB / T9341. The test results are shown in Tables 6 and 7.
[0141] Table 6
[0142] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Embodiment 13 <![CDATA[Impact strength / kJ / m 2 > 6.45 8.76 9.30 12.18 13.69 13.94 15.33 15.74 16.81 20.07
[0143] Table 7
[0144] Thionyl chloride Tetrabutyl titanate Benzenesulfonic acid KA1003 <![CDATA[17.08kJ / m 2 ]]> <![CDATA[16.89kJ / m 2 ]]> <![CDATA[17.46kJ / m 2 ]]> KBM-1003 <![CDATA[18.90kJ / m 2 ]]> <![CDATA[18.47kJ / m 2 ]]> <![CDATA[17.69kJ / m 2 ]]> KBM-403 <![CDATA[17.63kJ / m 2 ]]> <![CDATA[19.17kJ / m 2 ]]> <![CDATA[18.49kJ / m 2 ]]> X-12-817H <![CDATA[16.38kJ / m 2 ]]> <![CDATA[17.62kJ / m 2 ]]> <![CDATA[17.88kJ / m 2 ]]>
[0145] Aging test: After the composite material was aged in hot air at 100°C for 5 days, a tensile test was performed according to the above tensile test method and the tensile strength retention rate and elongation retention rate were calculated. The test results are shown in Tables 8 to 10. Table 9 shows the tensile strength retention rate of the PVC composite sheet obtained by the method of Examples 10-12 after the aging test. Table 10 shows the elongation retention rate of the PVC composite sheet obtained by the method of Examples 10-12 after the aging test.
[0146] Table 8
[0147] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Embodiment 13 Tensile strength retention rate / % 76 76 78 83 85 86 90 90 91 97 Elongation retention rate / % 70 71 75 81 82 82 87 89 89 95
[0148] Table 9
[0149] Thionyl chloride Tetrabutyl titanate Benzenesulfonic acid KA1003 91% 92% 92% KBM-1003 91% 92% 93% KBM-403 92% 93% 91% X-12-817H 90% 92% 91%
[0150] Table 10
[0151] Thionyl chloride Tetrabutyl titanate Benzenesulfonic acid KA1003 90% 89% 90% KBM-1003 89% 90% 88% KBM-403 90% 91% 91% X-12-817H 91% 91% 88%
[0152] From Tables 3 to 7, it can be seen that the addition of maleic acid and the addition of initiator in the curing process affect the performance of the product. The addition of the present invention can improve the mechanical properties of the composite material. The pretreatment of the glass and the lubricant layer can also improve the subsequent mechanical properties of the composite material. The optimal catalyst is tetrabutyl titanate and the silane coupling agent is KBM-403.
[0153] From Table 9 to Table 10, it can be seen that the multi-component system, raw material reaction sequence, and dosing operation in the curing reaction can improve the aging resistance of the product. The pre-treatment of glass fiber alone has little effect on the aging resistance of the product, but with the lubricating layer, the anti-aging effect is significantly improved.
[0154] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a glass fiber organic glass reinforced PVC composite sheet, characterized in that: include: S100, adding 400-500 parts of methyl methacrylate and 4-5 parts of initiator in a reaction kettle, uniformly heating to 80-100°C for 3.5-4.5 hours, then keeping the temperature constant for 1.5-2.5 hours, and finally cooling to below 30 degrees with frozen brine to obtain a prepolymer; S200, after uniformly mixing the glass fiber and the prepolymer, a curing process is performed to compound the glass fiber and the prepolymer to form glass fiber organic glass; S300, compounding the glass fiber organic glass and the PVC material through a hot pressing process to obtain a glass fiber organic glass reinforced PVC composite sheet; In parts by weight, the curing process comprises: adding 120-180 parts of glass fiber, 300-450 parts of prepolymer, 70-100 parts of maleic acid, 1.5-3 parts of emulsifier and 2-4 parts of initiator to 600-800 parts of methyl methacrylate, reacting at a temperature of 65-105° C. for 5-10 hours to obtain glass fiber organic glass, wherein the diameter of the glass fiber is 12-16 microns and the length is 0.25 mm-0.5 mm.
2. The method for preparing the glass fiber organic glass reinforced PVC composite sheet according to claim 1, characterized in that: In parts by weight, the addition operation of maleic acid in the curing process includes: adding 10-15 parts of maleic acid to the reaction system at one time, and then during the reaction of the system, first adding 10-25 parts of maleic acid at a uniform speed within 2-4 hours, then adding 40-65 parts of maleic acid at a uniform speed within 1-2 hours, and finally adding 10-20 parts of maleic acid at a uniform speed within 3-4 hours.
3. The method for preparing the glass fiber organic glass reinforced PVC composite sheet according to claim 2, characterized in that: In parts by weight, the addition operation of the initiator in the curing process includes: firstly adding 0.5-1 parts of the initiator at a uniform speed within 2-4 hours, and then adding 1.5-3 parts of the initiator at a uniform speed within 1-2 hours.
4. The method for preparing the glass fiber organic glass reinforced PVC composite sheet according to claim 1, characterized in that: The initiator includes one or more of azobisisobutyronitrile, benzoyl peroxide and a BPO / DMA mixed system, and the emulsifier includes one or more of OP-10, alkyl sulfate, polyoxyethylene ether and lecithin.
5. The method for preparing the glass fiber organic glass reinforced PVC composite sheet according to any one of claims 1 to 4, characterized in that: In parts by weight, the glass fiber is pretreated before being mixed with the prepolymer. The pretreatment operation includes: mixing 40-60 parts of maleic acid with 0.5-1.5 parts of a silane coupling agent to obtain a mixed solution with a pH value of 4-6, reacting the mixed solution at 50-60° C. for 1-2.5 hours, adding 80-100 parts of the glass fiber and 1-2 parts of a catalyst, and immersing the mixed solution at 60-70° C. for 5-8 hours to obtain the pretreated glass fiber.
6. The method for preparing the glass fiber organic glass reinforced PVC composite sheet according to claim 5, characterized in that: The catalyst includes one or more of thionyl chloride, tetrabutyl titanate and benzenesulfonic acid.
7. According to the method for preparing the glass fiber organic glass reinforced PVC composite plate material of claim 5, the silane coupling agent comprises one or more of KA1003, KBM-1003, KBM-403 and X-12-817H.
8. The method for preparing the glass fiber organic glass reinforced PVC composite sheet according to claim 5, characterized in that: A lubricating layer is formed on the surface of the pretreated glass fiber using calcium-based grease, and the hydrolysis temperature of the lubricating layer is 60-80°C.
9. A glass fiber organic glass reinforced PVC composite board prepared by the preparation method according to any one of claims 1 to 8.