An insulating and heat-conductive long carbon chain polyamide composition and preparation method thereof

By adopting hydroxylation treatment and two-dimensional thermal conductivity filler intercalation technology in the long carbon chain polyamide composition, combined with the combination of low-dimensional thermal conductivity fillers, the problem of difficult to take into account in the prior art is solved, and the problem of thermal conductivity and strength in the prior art is realized. Insulating thermally conductive long carbon chain polyamide composition with high thermal conductivity and high strength.

CN118685030BActive Publication Date: 2024-11-29ORINKO HIGH PERFORMANCE MATERIALS TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411166876.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The prior art is difficult to prepare an insulating thermally conductive long carbon chain polyamide composition with high thermal conductivity and high strength without reducing thermal conductivity.

Method used

The thermally conductive filler is treated by force chemistry to hydroxylate the surface. Combined with the combination technology of two-dimensional thermally conductive filler and low-dimensional thermally conductive filler, the two-dimensional thermally conductive filler is intercalated by molten alkali metal hydroxide to form a modified thermally conductive Filler and reinforcing fibers are added to the long carbon chain polyamide matrix.

Benefits of technology

The plane and normal thermal conductivity of the composition is significantly improved, while the overall mechanical properties are improved and the water absorption is reduced, achieving a balance of high thermal conductivity and high strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses an insulating thermally conductive long carbon chain polyamide composition and a preparation method thereof, and belongs to the technical field of modified materials. The insulating thermally conductive long carbon chain polyamide composition is prepared from the following raw materials by mass: 39.5-79.3 parts of long carbon chain polyamide, 20-40 parts of modified thermally conductive filler, 0-30 parts of reinforcing fiber, 0.3-3 parts of antioxidant, 0.2-3 parts of processing aid, 0.2-3 parts of masterbatch, the modified thermally conductive filler is a hydroxylated pre-treated thermally conductive filler, and the thermally conductive filler is a mixture of a two-dimensional thermally conductive filler and at least one low-dimensional thermally conductive filler. The present invention uses physical ball milling to treat the thermally conductive filler to hydroxylate its surface, thereby obtaining a modified thermally conductive filler, thereby weakening the agglomeration effect of the thermally conductive filler, improving the compatibility between the thermally conductive filler and the matrix resin, reducing the interfacial thermal resistance, and effectively improving the planar and normal thermal conductivity of the composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer material modification, and in particular to an insulating and heat-conductive long-carbon-chain polyamide composition and a preparation method thereof. Background Art

[0002] Battery cases, LED lighting housings, coil frames, etc. in traditional electric vehicles mostly use metal materials as heat dissipation materials, but metal materials are often heavy and not conducive to achieving product lightweighting.

[0003] The intrinsic thermal conductivity of conventional polymer materials is low, mainly concentrated in 0.15-0.4W / m·K. If they are to be used in the field of heat dissipation, they need to be thermally modified. There are currently two main methods to improve the thermal conductivity of polymer materials:

[0004] One is to improve the regularity of the polymer molecular chain structure, which is conducive to the close stacking of molecular chains, thereby improving the intrinsic thermal conductivity of the polymer. However, this method has a complex synthesis process, limited improvement effect, and the polymer processing performance is often poor.

[0005] The second method is to use polymer materials as the matrix, fill them with thermal conductive fillers to prepare filled polymer-based thermal conductive composite materials, and adjust the distribution of thermal conductive fillers in the matrix to form a continuous thermal conductive path, thereby improving the thermal conductivity of the system. This method has a simple production process and is more feasible.

[0006] Polyamide (PA) is the most widely used engineering plastic at present. It has strong crystallinity, high mechanical strength, good processing flowability and strong corrosion resistance, making it very suitable as a matrix for thermal conductive composite materials. Among them, long-chain polyamide (LCPA) has a long methylene segment between adjacent amide groups. In addition to the basic properties of polyamide, it also has the characteristics of low relative density and low water absorption, making it an ideal matrix for thermal conductive polymer materials.

[0007] At present, there are reports on thermal conductivity modification of long carbon chain polyamides. For example, patent CN107057338A uses 10-25% carbon material and 5-20% metal indium to construct a conductive and thermal network path in nylon composite materials; patent CN113150541A uses graphene nylon masterbatch, 5-30 parts of carbon fiber and 10-30 parts of thermal conductive filler to prepare a high-strength and high-thermal conductivity nylon composite material. Although the metal material or carbon material has a high thermal conductivity coefficient and can significantly improve the thermal conductivity of the composition at a lower filling ratio, the composition is often not insulating.

[0008] In order to prepare an insulating and thermally conductive long-chain polyamide composition, a large amount of ceramic-based high thermal conductivity fillers need to be filled in the matrix. For example, patent CN104744935A uses 30-50% boron nitride, magnesium oxide, aluminum oxide and other thermally conductive fillers to prepare a long carbon chain thermally conductive nylon composite material. However, the compatibility of ceramic-based thermally conductive fillers with the resin matrix is ​​poor, and the interfacial bonding force is weak. At the same time, due to the small size effect of ceramic-based thermally conductive fillers, it is easy to agglomerate in the polymer, which is not conducive to the overlap of the thermally conductive filler network. Therefore, some additives are often used to surface treat the thermally conductive filler to improve its compatibility with the matrix. However, if the amount of additives added is too much, it will cause interfacial thermal resistance to the thermal conductivity of the composite material, reducing the thermal conductivity of the system.

[0009] Therefore, how to prepare an insulating and thermally conductive long-chain polyamide composition with high thermal conductivity and high strength is a difficult problem of great practical significance. Summary of the invention

[0010] In order to solve the problems existing in the prior art, the present invention discloses an insulating and heat-conductive long-carbon-chain polyamide composition and a preparation method thereof.

[0011] The specific technical solutions of the present invention are as follows:

[0012] The first object of the present invention is to provide an insulating and heat-conductive long carbon chain polyamide composition, which is prepared from the following raw materials in parts by mass:

[0013] 39.5 to 79.3 parts of long carbon chain polyamide,

[0014] 20-40 parts of modified thermal conductive filler,

[0015] Reinforcement fiber 0-30 parts,

[0016] 0.3-3 parts of antioxidant,

[0017] Processing aid 0.2-3 parts,

[0018] Masterbatch 0.2-3 parts,

[0019] The modified thermally conductive filler is a thermally conductive filler pretreated by hydroxylation, and the thermally conductive filler is a mixture of a two-dimensional thermally conductive filler and at least one low-dimensional thermally conductive filler.

[0020] In a further embodiment, the low-dimensional thermally conductive filler is a zero-dimensional thermally conductive filler and / or a one-dimensional thermally conductive filler;

[0021] The zero-dimensional thermal conductive filler includes powdered aluminum nitride, silicon nitride, aluminum oxide, magnesium oxide or zinc oxide;

[0022] The one-dimensional thermal conductive filler includes needle-shaped wollastonite or zinc oxide whiskers.

[0023] In a further embodiment, the two-dimensional thermally conductive filler is hexagonal boron nitride (h-BN).

[0024] In a further embodiment, the preparation method of the modified thermally conductive filler is as follows:

[0025] (1) placing a two-dimensional thermally conductive filler and an alkali metal hydroxide in a reaction kettle and heating them to perform alkali intercalation to obtain an intercalated two-dimensional thermally conductive filler; and then dispersing the intercalated two-dimensional thermally conductive filler in water to obtain a suspension;

[0026] (2) adding a low-dimensional thermally conductive filler to the suspension prepared in step (1) and mixing the mixture to obtain a mixed solution;

[0027] (3) The mixed liquid is added to a ball mill for ball milling to obtain a uniform mixed dispersion, which is then filtered and washed with water until the filtrate is neutral and then dried to obtain a modified thermal conductive filler.

[0028] In a further embodiment, the alkali metal hydroxide in step (1) is NaOH and KOH; the mass ratio of the two-dimensional thermal conductive filler, NaOH and KOH is 1:2-3:2-3;

[0029] The heating temperature is 170-190° C. and the heating time is 1.5-2.5 hours.

[0030] In a further embodiment, the mass ratio of the two-dimensional thermally conductive filler to the low-dimensional thermally conductive filler in step (2) is 3-1:1-7.

[0031] In a further embodiment, the volume ratio of the mixed liquid to the ball milling medium in the ball mill is 1:0.5-0.8;

[0032] The ball milling is carried out continuously at 200-500 rpm for 10-20 hours.

[0033] In a further embodiment, the long carbon chain polyamide has a melt index of 15 to 35 g / 10 min at 235° C. / 2.16 kg.

[0034] In a further embodiment, the long carbon chain polyamide is at least one of PA510, PA512, PA513, PA514, PA515, PA610, PA612, PA613, PA614, PA615, PA1010, PA1012, PA1013, PA1014, PA1015, PA11, PA12, PA1212, PA1213, PA1214, and PA1215.

[0035] In a further embodiment, the reinforcing fiber is at least one of basalt fiber and glass fiber.

[0036] In a further embodiment, the antioxidant is at least one of a hindered phenol antioxidant, an amine antioxidant, a phosphite antioxidant, and a thioester antioxidant.

[0037] In a further embodiment, the processing aid is at least one of ethylene bisstearamide (EBS), silicone masterbatch, anti-glass fiber exposure agent (TAF), and pentaerythritol stearate (PETS);

[0038] The masterbatch is at least one of a PA masterbatch and a PE masterbatch.

[0039] The second object of the present invention is to provide a method for preparing the above-mentioned insulating heat-conductive long carbon chain polyamide composition, which comprises the following steps:

[0040] S1. Weigh long carbon chain polyamide, modified thermal conductive filler, antioxidant, processing aid, and masterbatch according to the formula mass parts, place them in a high-speed mixer and stir for 3 to 10 minutes to obtain a mixed material;

[0041] S2, adding the mixed material into the main feeding port of the twin-screw extruder, adding the reinforcing fiber into the side feeding port, and after melting, extrusion, pelletizing and drying, the obtained product is obtained.

[0042] In a further embodiment, the temperature of one zone of the twin-screw extruder is 150-190° C., and the temperature of other zones and the die head is 180-260° C.; the screw speed is 200-600 r / min.

[0043] The present invention uses a mechanochemical method (i.e., physical ball milling) to treat the thermally conductive filler to hydroxylate its surface, thereby obtaining a modified thermally conductive filler, thereby weakening the agglomeration effect of the thermally conductive filler, improving the compatibility between the thermally conductive filler and the matrix resin, reducing the interface thermal resistance, and effectively improving the thermal conductivity of the composition.

[0044] The thermally conductive filler in the present invention is a mixture of at least one of a two-dimensional thermally conductive filler and a low-dimensional thermally conductive filler (including a zero-dimensional thermally conductive filler and a one-dimensional thermally conductive filler), wherein the two-dimensional thermally conductive filler is subjected to a melt intercalation treatment with an alkali metal hydroxide to obtain a two-dimensional lamellar structure; a zero-dimensional thermally conductive filler refers to a granular or powdered form that occupies only a very small volume in the spatial dimension, such as aluminum nitride, silicon nitride, aluminum oxide, magnesium oxide, zinc oxide, etc.; a one-dimensional thermally conductive filler refers to those fillers that extend mainly in one direction in the spatial dimension, such as needle-shaped wollastonite, zinc oxide whiskers, etc. Therefore, this application selects different types and shapes of thermally conductive fillers of multiple sizes for compound use. Small-sized thermally conductive fillers can be filled between large-sized thermally conductive fillers, thereby improving the efficiency of building a thermally conductive path, so that the construction of a complete thermally conductive path in the composition can be completed with a smaller filling amount, significantly improving the planar and normal thermal conductivity of the composition.

[0045] The present invention uses molten alkali metal hydroxide to perform intercalation treatment on the two-dimensional thermal conductive filler h-BN. Driven by high chemical potential, metal ions and OH- are inserted into the interlayer of h-BN, and then diffuse into the space between adjacent BN lattices, causing the top h-BN layer to curl or wrinkle. When more ions enter the interlayer space, the curled sheets are peeled off from the matrix, thereby obtaining a complete two-dimensional lamellar structure; the two-dimensional thermal conductive filler is well dispersed and a thermal conductive path can be constructed at a low content, thereby significantly improving the thermal conductivity of the composition.

[0046] Therefore, the present invention improves the compatibility of the filler and the matrix through the synergistic effect of the hydroxylated multi-dimensional thermally conductive filler, realizes the construction of a perfect thermal conductive path at a lower filling amount in the composition, and simultaneously improves the planar and normal thermal conductivity of the composition.

[0047] In addition, the present invention improves the overall mechanical properties of the composition, improves dimensional stability, reduces the water absorption of the composition, and promotes the construction of a heat conduction path by adding reinforcing fibers.

[0048] The ball milling medium used in the present invention is composed of a mixture of zirconia balls with a diameter of 2 mm and zirconia balls with a diameter of 8 mm in a mass ratio of 0-4:1-5. During ball milling, the volume ratio of the mixed liquid to the ball milling medium is 1:0.5-0.8. The compound use of ball milling media of different sizes can play a role in shearing and peeling the intercalated two-dimensional thermal conductive filler. At the same time, in an alkaline solution environment, the surface of the filler can be hydroxylated during the shearing process of the ball milling medium and the thermal conductive filler, that is, the filler functionalization is completed by a mechanochemical method. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is described in detail below through specific embodiments. The following embodiments are only used to further illustrate the present invention and are not intended to limit the protection scope of the present invention.

[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for describing specific embodiments and are not intended to limit the present invention.

[0051] The specific information of the raw materials used in the following examples and comparative examples is shown in Table 1. Products produced by other manufacturers are also suitable for the present invention.

[0052] Table 1. Raw material information

[0053]

[0054] All materials are conventional commercial products. The above raw materials and reagents are only examples of some specific embodiments of the present invention, and do not mean that the present invention can only use the above reagents. The specific scope shall be subject to the scope in the claims.

[0055] Embodiment 1:

[0056] S1. Preparation of modified thermal conductive filler:

[0057] (1) 10 kg of two-dimensional thermal conductive filler h-BN, NaOH and KOH were placed in a polytetrafluoroethylene-lined reactor and heated at 170°C for 2.5 hours for melt-alkali intercalation. After completion, the mixture was cooled to room temperature to obtain an intercalated two-dimensional thermal conductive filler. The intercalated two-dimensional thermal conductive filler was then dispersed in water to obtain a suspension. The mass ratio of h-BN, NaOH, KOH and water was 1:2:2:100.

[0058] (2) adding 10 kg of magnesium oxide and 8 kg of zinc oxide whiskers to the suspension prepared in step (1) and mixing them evenly to obtain a mixed solution; and maintaining the mass ratio of all thermal conductive fillers to NaOH, KOH, and water to be 1:2:2:100;

[0059] (3) Add the mixed solution into a ball mill and continuously ball mill at 200 rpm for 20 hours to obtain a uniform mixed dispersion, and then filter and wash with water until the filtrate is neutral and then dry to obtain a modified thermal conductive filler;

[0060] The volume ratio of the mixed liquid to the ball milling medium in the ball mill is 1:0.5; the ball milling medium is composed of zirconia balls with a diameter of 2 mm and zirconia balls with a diameter of 8 mm mixed in a mass ratio of 4:1.

[0061] S2. According to the formula and weight parts in Table 1, long carbon chain polyamide, modified thermal conductive filler, antioxidant, processing aid, and masterbatch were weighed and placed in a high-speed mixer and stirred for 3 minutes to obtain a mixed material;

[0062] S3, adding the mixed material into the main feeding port of the twin-screw extruder, adding the reinforcing fiber into the side feeding port, and after melting, extrusion, pelletizing and drying, the obtained product is obtained.

[0063] The temperature of one zone of the twin-screw extruder is 150°C, and the temperature of other zones and the die head is 230°C; the screw speed is 200r / min.

[0064] Embodiment 2:

[0065] The preparation method is the same as that of Example 1, except that some components and amounts are different, as shown in Table 2.

[0066] Embodiment 3:

[0067] S1. Preparation of modified thermal conductive filler:

[0068] (1) 10 kg of two-dimensional thermal conductive filler h-BN, NaOH and KOH were placed in a polytetrafluoroethylene-lined reactor and heated at 190°C for 1.5 hours to perform alkali intercalation. After completion, the mixture was cooled to room temperature to obtain an intercalated two-dimensional thermal conductive filler. The intercalated two-dimensional thermal conductive filler was then dispersed in water to obtain a suspension. The mass ratio of h-BN, NaOH, KOH and water was 1:3:3:100.

[0069] (2) adding 18 kg of magnesium oxide to the suspension prepared in step (1) and mixing them evenly to obtain a mixed solution; wherein the mass ratio of h-BN to the low-dimensional thermal conductive filler is 1:1.8; and the mass ratio of all the thermal conductive fillers to NaOH, KOH, and water is still 1:3:3:100;

[0070] (3) Add the mixed solution into a ball mill and continuously ball mill at 500 rpm for 10 hours to obtain a uniform mixed dispersion, and then filter and wash with water until the filtrate is neutral and then dry to obtain a modified thermal conductive filler;

[0071] The volume ratio of the mixed liquid to the ball milling medium in the ball mill is 1:0.8; the ball milling medium is composed of zirconia balls with a diameter of 2 mm and a diameter of 8 mm in a mass ratio of 1:4.

[0072] S2. Weigh the long carbon chain polyamide, modified thermal conductive filler, antioxidant, processing aid, and masterbatch according to the formula in Table 1, place them in a high-speed mixer and stir for 10 minutes to obtain a mixed material;

[0073] S3, adding the mixed material into the main feeding port of the twin-screw extruder, adding the reinforcing fiber into the side feeding port, and after melting, extrusion, pelletizing and drying, the obtained product is obtained.

[0074] The temperature of one zone of the twin-screw extruder is 190°C, and the temperature of other zones and the die head is 260°C; the screw speed is 600r / min.

[0075] Embodiment 4,5:

[0076] The preparation method is the same as that of Example 1, except that some components and amounts are different, as shown in Table 2.

[0077] Embodiment 6, 7:

[0078] The preparation method is the same as that of Example 3, except that some components and amounts are different, as shown in Table 2.

[0079] Comparative Example 1:

[0080] The preparation method is the same as that of Example 1, except that the modified thermal conductive filler is different. The preparation method is as follows:

[0081] (1) Add 28 kg of magnesium oxide to an aqueous solution of NaOH and KOH so that the mass ratio of magnesium oxide to NaOH, KOH and water is 1:2:2:100;

[0082] (2) Add the mixed solution to a ball mill and continuously ball mill at 500 rpm for 10 hours to obtain a uniform mixed dispersion, and then filter and wash with water until the filtrate is neutral and then dry to obtain a modified thermal conductive filler;

[0083] The volume ratio of the mixed liquid to the ball milling medium in the ball mill is 1:0.5; the ball milling medium is composed of zirconia balls with a diameter of 2 mm and zirconia balls with a diameter of 8 mm mixed in a mass ratio of 4:1.

[0084] Comparative Example 2:

[0085] The same as comparative example 1, except that the modified thermal conductive filler is modified with respect to 28 kg of zinc oxide whiskers.

[0086] Comparative Example 3:

[0087] Same as Example 1, the only difference is that the thermal conductive filler is different (not modified), and the preparation method is as follows:

[0088] (1) 10 kg of two-dimensional thermal conductive filler h-BN, NaOH and KOH were placed in a polytetrafluoroethylene-lined reactor and heated at 170°C for 2.5 hours for melt-alkali intercalation, and then cooled to room temperature to obtain an intercalated two-dimensional thermal conductive filler;

[0089] (2) Add 10 kg of magnesium oxide and 8 kg of zinc oxide whiskers and mix evenly to obtain a thermal conductive filler.

[0090] Comparative Example 4:

[0091] Same as Example 5, the only difference is that the thermal conductive filler is different (h-BN is not intercalated), and the preparation method is as follows:

[0092] (1) Add 15 kg of two-dimensional thermal conductive filler h-BN and 5 kg of zinc oxide whiskers into NaOH and KOH aqueous solutions and mix them evenly to obtain a mixed solution; the mass ratio of h-BN to the low-dimensional thermal conductive filler is 3:1; and the mass ratio of all thermal conductive fillers to NaOH, KOH, and water is still 1:2:2:100;

[0093] (2) Add the mixed solution into a ball mill and continuously ball mill at 200 rpm for 20 hours to obtain a uniform mixed dispersion, and then filter and wash with water until the filtrate is neutral and then dry to obtain a modified thermal conductive filler;

[0094] The volume ratio of the mixed liquid to the ball milling medium in the ball mill is 1:0.5; the ball milling medium is composed of zirconia balls with a diameter of 2 mm and zirconia balls with a diameter of 8 mm mixed in a mass ratio of 4:1.

[0095] Comparative Example 5:

[0096] The same as Example 4, except that the modified thermal conductive filler is different (no two-dimensional thermal conductive filler h-BN is added), and the preparation method is as follows:

[0097] (1) Add 15 kg of magnesium oxide, 10 kg of aluminum oxide, and 15 kg of zinc oxide whiskers into NaOH and KOH aqueous solutions, mix them evenly to obtain a mixed solution; the mass ratio of all thermal conductive fillers to NaOH, KOH, and water is 1:2:2:100;

[0098] (2) Add the mixed solution into a ball mill and continuously ball mill at 200 rpm for 20 hours to obtain a uniform mixed dispersion, and then filter and wash with water until the filtrate is neutral and then dry to obtain a modified thermal conductive filler;

[0099] The volume ratio of the mixed liquid to the ball milling medium in the ball mill is 1:0.5; the ball milling medium is composed of zirconia balls with a diameter of 2 mm and zirconia balls with a diameter of 8 mm mixed in a mass ratio of 4:1.

[0100] Comparative Example 6:

[0101] The same as Example 5, except that the modified thermal conductive filler was ball-milled at 1000 rpm for 20 hours.

[0102] Comparative Example 7:

[0103] Same as Example 7, the only difference is that the thermal conductive filler is different (only the intercalated two-dimensional thermal conductive filler is added), and no reinforcing fiber is added. The preparation method of the intercalated two-dimensional thermal conductive filler is as follows:

[0104] 20 kg of two-dimensional thermal conductive filler h-BN, NaOH and KOH were placed in a polytetrafluoroethylene-lined reactor and heated at 180°C for 2 hours for melt-alkali intercalation. After the intercalation, it was cooled to room temperature to obtain an intercalated two-dimensional thermal conductive filler; the mass ratio of h-BN, NaOH, KOH and water was 1:2:3:100.

[0105] The specific formulas of the above Examples 1-7 and Comparative Examples 1-7 are shown in Table 2 below:

[0106] Table 2. Formula and dosage (unit: kg)

[0107]

[0108] After homogenization treatment, the insulating and thermally conductive long carbon chain polyamide composition particles obtained in the above Examples 1-7 and Comparative Examples 1-7 were injection molded into specimens and subjected to performance tests. The test items and results are shown in Tables 3 and 4.

[0109] Table 3. Performance test results of the compositions prepared in Examples 1-7

[0110]

[0111] Table 4. Performance test results of the compositions prepared in Comparative Examples 1-7

[0112]

[0113] The test standards for the above test items are as follows:

[0114] (1) Tensile strength test standard reference: GB / T 1040.2-2006;

[0115] (2) Bending strength test standard reference: GB / T 9341-2008;

[0116] (3) Simply supported beam notched impact strength test standard reference: GB / T 1043.1-2008;

[0117] (4) Water absorption test standard reference: GB / T 1034-2008;

[0118] (5) Thermal conductivity test standard reference: GB / T 22588-2008;

[0119] (6) Thermal deformation temperature test standard reference: GB / T 1634.2-2004;

[0120] (7) Volume resistivity test standard reference: GB / T 31838.2-2019.

[0121] According to the test results in Tables 3 and 4, the plane thermal conductivity of the insulating heat-conductive long carbon chain polyamide compositions prepared in Examples 1 to 7 of the present invention is not less than 2.0 W / (m·K), the normal thermal conductivity is not less than 0.8 W / (m·K), and the volume resistivity is greater than 10 10 Ω·m. Therefore, the composition prepared by the present invention has good thermal conductivity and insulation properties.

[0122] A comprehensive comparison of Example 1 and Comparative Examples 1 to 2 shows that the two-dimensional thermally conductive filler and the low-dimensional thermally conductive filler in Example 1 are used in combination, and the strength, water absorption rate and other properties of the composition do not change much compared to using the same number of zero-dimensional thermally conductive fillers or one-dimensional thermally conductive fillers alone; however, the thermal conductivity of the composition is significantly improved. This is because the boron nitride sheet structure with a two-dimensional structure is easy to orient in the plane, and when compounding zero-dimensional and / or one-dimensional fillers, the layers of the two-dimensional boron nitride can overlap with each other, thereby improving the efficiency of building the thermal conductive path, so that the composition has a complete thermal conductive path in both the planar direction and the normal direction, effectively improving the thermal conductivity of the composition.

[0123] A comprehensive comparison of Example 4 and Comparative Example 5 also shows that the absence of the two-dimensional thermally conductive filler significantly leads to a decrease in the thermal conductivity of the composition plane, indicating that the two-dimensional thermally conductive filler plays an important role in the construction of the thermal conductive path in the composition.

[0124] A comprehensive comparison of Example 7 and Comparative Example 7 shows that when 20 parts of the two-dimensional thermally conductive filler h-BN are added alone, the in-plane thermal conductivity of the composition is 2.3 W / (m·K), and the normal thermal conductivity is 0.6 W / (m·K); when 20 parts of h-BN are compounded with 10 parts of aluminum nitride and 20 parts of reinforcing fibers, the in-plane thermal conductivity of the composition is increased to 3.1 W / (m·K), and the normal thermal conductivity is increased to 1.4 W / (m·K), proving that the compounding of the two-dimensional thermally conductive filler h-BN and the low-dimensional thermally conductive filler can synergistically improve the in-plane and normal thermal conductivity of the composition.

[0125] A comprehensive comparison of Example 1 and Comparative Example 3 shows that the addition of the modified thermally conductive filler improves the strength of the composition and significantly improves the thermal conductivity compared to the addition of the same amount of unmodified thermally conductive filler. This is because the hydroxylated modified thermally conductive filler can improve the filler agglomeration problem, improve the compatibility of the filler with the matrix, and reduce the interface thermal resistance, which is of great value to the improvement of the strength and thermal conductivity of the composition.

[0126] A comprehensive comparison of Example 5 and Comparative Examples 4 and 6 shows that the two-dimensional thermally conductive filler in Comparative Example 4 was added without modification by molten alkali intercalation, and the modified filler in Comparative Example 6 was milled at too high a speed during the preparation process, and the thermal conductivity was lower than that of the composition prepared in Example 5 of the present invention. This is because the modified thermally conductive filler was first treated by molten alkali intercalation and then subjected to appropriate ball milling treatment, which helps to obtain thin and complete hydroxylated two-dimensional sheets, which is very effective in improving the thermal conductivity of the composition.

[0127] A comprehensive comparison of Example 1 and Example 2 shows that the addition of reinforcing fibers improves the overall mechanical properties of the composition, improves dimensional stability, and reduces the water absorption of the composition. At the same time, the one-dimensional structure of the reinforcing fibers also promotes the construction of a heat conduction path in the system.

[0128] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An insulating and heat-conductive long carbon chain polyamide composition, characterized in that: It is prepared from the following raw materials by mass: 39.5 to 79.3 parts of long carbon chain polyamide, 20-40 parts of modified thermal conductive filler, Reinforcement fiber 0-30 parts, 0.3-3 parts of antioxidant, Processing aid 0.2-3 parts, Masterbatch 0.2-3 parts, The modified thermally conductive filler is a thermally conductive filler pretreated by hydroxylation, the thermally conductive filler is a mixture of a two-dimensional thermally conductive filler, a zero-dimensional thermally conductive filler and a one-dimensional thermally conductive filler, and the zero-dimensional thermally conductive filler and the one-dimensional thermally conductive filler are low-dimensional thermally conductive fillers; The preparation method of the modified thermally conductive filler is as follows: (1) placing a two-dimensional thermally conductive filler and an alkali metal hydroxide in a reaction kettle and heating them to perform alkali intercalation to obtain an intercalated two-dimensional thermally conductive filler; and then dispersing the intercalated two-dimensional thermally conductive filler in water to obtain a suspension; (2) adding a low-dimensional thermally conductive filler to the suspension prepared in step (1) and mixing the mixture to obtain a mixed solution; (3) Add the mixed liquid to a ball mill and continuously ball mill at 200-500 rpm for 10-20 hours to obtain a uniform mixed dispersion, and then filter and wash with water until the filtrate is neutral and then dry to obtain a modified thermal conductive filler; The zero-dimensional thermal conductive filler includes powdered aluminum nitride, silicon nitride, aluminum oxide, magnesium oxide or zinc oxide; The one-dimensional thermal conductive filler includes needle-shaped wollastonite or zinc oxide whiskers; The two-dimensional thermal conductive filler is hexagonal boron nitride.

2. The insulating and heat-conductive long carbon chain polyamide composition according to claim 1, characterized in that: The alkali metal hydroxides in step (1) are NaOH and KOH; the mass ratio of the two-dimensional thermal conductive filler, NaOH and KOH is 1:2-3:2-3; The heating temperature is 170-190° C. and the heating time is 1.5-2.5 hours.

3. The insulating and heat-conductive long carbon chain polyamide composition according to claim 1, characterized in that: The mass ratio of the two-dimensional thermally conductive filler to the low-dimensional thermally conductive filler in step (2) is 3-1:1-7.

4. The insulating and heat-conductive long carbon chain polyamide composition according to claim 1, characterized in that: The volume ratio of the mixed liquid to the ball milling medium in the ball mill is 1:0.5-0.

8.

5. The insulating and thermally conductive long carbon chain polyamide composition according to claim 1, characterized in that: The long carbon chain polyamide has a melting index of 15 to 35 g / 10 min at 235° C. / 2.16 kg.

6. The insulating and thermally conductive long carbon chain polyamide composition according to claim 5, characterized in that: The long carbon chain polyamide is at least one of PA510, PA512, PA513, PA514, PA515, PA610, PA612, PA613, PA614, PA615, PA1010, PA1012, PA1013, PA1014, PA1015, PA11, PA12, PA1212, PA1213, PA1214, and PA1215.

7. The insulating and thermally conductive long carbon chain polyamide composition according to claim 1, characterized in that: The reinforcing fiber is at least one of basalt fiber and glass fiber.

8. The insulating and thermally conductive long carbon chain polyamide composition according to claim 1, characterized in that: The antioxidant is at least one of a hindered phenol antioxidant, an amine antioxidant, a phosphite antioxidant, and a thioester antioxidant.

9. The insulating and thermally conductive long carbon chain polyamide composition according to claim 1, characterized in that: The processing aid is at least one of ethylene bis stearamide, silicone masterbatch, anti-glass fiber exposure agent, and pentaerythritol stearate; The masterbatch is at least one of a PA masterbatch and a PE masterbatch.

10. A method for preparing an insulating and heat-conductive long carbon chain polyamide composition according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Weigh long carbon chain polyamide, modified thermal conductive filler, antioxidant, processing aid, and masterbatch according to mass, place in a high-speed mixer and stir for 3 to 10 minutes to obtain a mixed material; S2, adding the mixed material into the main feeding port of the twin-screw extruder, adding the reinforcing fiber into the side feeding port, and after melting, extrusion, pelletizing and drying, the obtained product is obtained.

11. The preparation method according to claim 10, characterized in that: The temperature of one zone of the twin-screw extruder is 150-190° C., and the temperatures of other zones and the die are 180-260° C.; the screw speed is 200-600 r / min.

Citation Information

Patent Citations

  • Long-carbon-chain heat-conducting nylon composite material and preparation method thereof

    CN104744935A

  • Electromagnetic shielding nylon composite material with high thermal conductivity for battery box of new energy automobile

    CN107057338A

  • High-strength high-thermal-conductivity nylon composite material and preparation method thereof

    CN113150541A

  • High-whiteness, halogen-free, flame-retardant, thermal conductive and insulated PA 6 (polyamide 6)-based composite material and preparation method thereof

    CN103709740A

  • Heat-conducting ceramic silicone rubber material and preparation method thereof

    CN113105743A

Cited By

  • Polyamide composite material as well as preparation method and application thereof

    CN120158082A

  • Polyamide composite material and preparation method and application thereof

    CN120158082B