A method for extrusion casting of intelligent metal parts with embedded sensors
By using the extrusion casting method of TPMS bionic structure in smart metal parts to package the fiber Bragg grating sensor in one step, the problem of the sensor being easily damaged in harsh environments and complex packaging is solved, achieving high precision, low cost and strong stability. Smart metal parts.
Patent Information
- Application Number
- CN202411200884.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-29
AI Technical Summary
In the existing technology, fiber Bragg grating sensors are easily damaged in harsh environments, and the sensor packaging process is complicated and requires multiple packaging to ensure that it is not damaged during operation, resulting in high material costs and complex process flows.
Using the extrusion casting method of smart metal parts with embedded sensors, a porous rod frame with a three-period minimal surface (TPMS) bionic structure is prepared, the optical fiber sensor is penetrated into the preset structural health detection position, and added to the extrusion mold The molten aluminum alloy is subjected to one-step packaging by applying pressure to complete the metallurgical bonding of dissimilar metal materials.
It achieves high sample precision, easy control of structural orientation, saves material costs, simplifies the packaging process, improves the service life stability of the fiber Bragg grating sensor, and avoids damage to the sensor in harsh environments.
Smart Images

Figure CN118699335B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of casting, and in particular to an extrusion casting method for an intelligent metal part with an embedded sensor. Background Art
[0002] With the rapid development of modern industry, a single material can no longer meet the diversified technical requirements. With the advent of intelligence in various fields, the demand for health status detection of mechanical components is also increasing, and the material field is gradually developing towards composite materials and intelligent materials. Fiber Bragg grating (FBG) sensors have the advantages of small size, anti-interference, and easy to form a sensor network. They have important applications in the field of structural health detection. However, bare optical fibers are very fragile and easily damaged in harsh environments. Smart metal parts with embedded sensors integrate heterogeneous material composite technology and sensor packaging technology to embed FBG sensors into titanium / aluminum composite materials. Due to the large difference in the properties of the two selected metals, the strong and tough alternating arrangement of natural biological support materials is met, and the selected rod frame structure is a three-periodic minimal surface (TPMS) found in biological bones. Therefore, the strength and toughness of biomimetic properties are synergistically improved on the three-dimensional interpenetrating structure, which greatly protects the FBG sensors in harsh working environments. In the existing sensor packaging technology, due to the fragility of fiber Bragg grating (FBG) sensors, it is usually necessary to perform two packagings, one at the primary level and the other at the secondary level, before preparing the parts to ensure that the sensors are not damaged during operation. The sensor packaging process is complicated. Summary of the invention
[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to propose an extrusion casting method for intelligent metal parts with embedded sensors. The fiber Bragg grating (FBG) sensor is embedded and packaged by means of quantitative extrusion casting, and the metallurgical bonding of dissimilar metal materials is completed at the same time, so as to prepare the intelligent metal parts with embedded sensors in one step.
[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0005] A method for extrusion casting of a smart metal part with an embedded sensor, comprising the following steps:
[0006] S1. Preparation of a porous rod frame with a TPMS bionic structure;
[0007] S2. Selecting a preset structural health detection position for the porous rod frame, inserting the optical fiber sensor into the preset structural health detection position, and placing it into the extrusion die;
[0008] S3. Add aluminum alloy melt into the extrusion die, then control the pressure head to apply pressure, maintain the pressure for a certain period of time and then cool it to obtain a smart metal part with an embedded sensor.
[0009] As a preferred embodiment of the extrusion casting method of a smart metal part with an embedded sensor described in the present invention, in which: in step S1, the porous rod frame is a porous titanium alloy rod frame or a porous stainless steel rod frame; the titanium alloy is Ti-6Al-4V titanium alloy, and the stainless steel is 316L stainless steel.
[0010] As a preferred embodiment of the extrusion casting method of a smart metal part with an embedded sensor described in the present invention, in which: in the step S1, a porous rod frame with a TPMS bionic structure is prepared by an additive manufacturing process, and the specific process is: using Matlab software to establish a three-dimensional model of a three-periodic minimal surface (TPMS) through implicit trigonometric functions, importing it into Materialise Magics 23.0, setting the parameters of the TPMS structure, then creating a new processing platform in Materialise Magics23.0, dragging the part to the substrate, and slicing it. Secondly, opening the EPHatch software in the additive manufacturing equipment, saving the slices, and completing the operation on the computer; then performing equipment and machine interface operations, setting additive manufacturing process parameters, and finally filling the powder bin with alloy powder and protective gas for additive manufacturing.
[0011] As a preferred embodiment of the extrusion casting method of an intelligent metal part with an embedded sensor described in the present invention, in which: in the step S1, the porous rod frame is placed in a NaOH solution with a concentration of 10-20wt% for alkaline washing for 5-10 minutes to remove oil stains on the surface of the titanium alloy, and then the porous rod frame is placed in a hydrochloric acid solution with a concentration of 10-20wt% for pickling for 5-10 minutes to remove rust and other oxide layers of the porous rod frame, and finally cleaned with alcohol to achieve a cleanliness that meets the casting requirements.
[0012] As a preferred embodiment of the extrusion casting method of an intelligent metal part with an embedded sensor described in the present invention, wherein: in the step S1, the cleaned porous titanium alloy rod frame is placed in a plating aid solution of 8.3wt%K2ZrF6-8.3wt%KCl-0.08wt%NaF at a temperature of 85-95°C for 5-10 minutes, then taken out and placed in an oven at 195-205°C for drying for 30 minutes to complete the plating aid treatment. The plating aid forms a salt film on the surface of the titanium alloy to prevent the titanium alloy from being exposed to air and being oxidized, and to maintain the surface activity of the porous titanium alloy rod frame.
[0013] As a preferred embodiment of the extrusion casting method of an intelligent metal part with an embedded sensor described in the present invention, in which: in the step S1, the cleaned porous stainless steel rod frame is placed in a 6wt%KF-2wt%ZnCl2 plating aid solution at a temperature of 65~75°C for 15~20 minutes, then taken out and placed in an oven at 105~115°C for drying for 15 minutes to complete the plating aid treatment.
[0014] As a preferred embodiment of the extrusion casting method of a smart metal part with an embedded sensor described in the present invention, in the step S2, the selection of the health detection position must meet two points: first, surround and support the optical fiber sensor to prevent damage to the optical fiber sensor caused by high pressure during extrusion casting; second, position the optical fiber sensor, fix the optical fiber sensor using the TPMS structural units arranged in a regular periodic manner, and locate the position for the sensor health detection.
[0015] As a preferred solution of the extrusion casting method of a smart metal part with an embedded sensor described in the present invention, wherein: in the step S2, the optical fiber sensor is a high-temperature femtosecond metal-clad optical fiber Bragg grating sensor.
[0016] As a preferred solution of the extrusion casting method of a smart metal part with an embedded sensor described in the present invention, in the step S2, both ends of the optical fiber are left outside the mold to facilitate the collection of subsequent detection signals.
[0017] As a preferred embodiment of the extrusion casting method of an intelligent metal part with an embedded sensor described in the present invention, in which: in the step S3, the extrusion die is preheated to prevent the aluminum alloy melt from being quenched and destroying the bonding interface. When the die temperature reaches 200-400°C, a preset weight of aluminum alloy melt is added to the extrusion die through an electromagnetic quantitative conveying device.
[0018] As a preferred embodiment of the extrusion casting method of a smart metal part with an embedded sensor described in the present invention, in step S3, the pressure is 150-180 MPa and the pressure is maintained for 30-60 seconds.
[0019] As a preferred embodiment of the extrusion casting method of a smart metal part with an embedded sensor described in the present invention, in step S3, the aluminum alloy is an Al-Si alloy.
[0020] As a preferred embodiment of the extrusion casting method of a smart metal part with an embedded sensor described in the present invention, in step S3, the smart metal part with an embedded sensor can obtain stress, strain and temperature values of the test part through feedback signals.
[0021] The beneficial effects of the present invention are as follows:
[0022] The present invention proposes an extrusion casting method for smart metal parts with embedded sensors, preparing a porous rod frame with a TPMS bionic structure; selecting a preset structural health detection position for the porous rod frame, inserting the optical fiber sensor into the preset structural health detection position, and placing it in an extrusion die; adding aluminum alloy melt to the extrusion die, then controlling the pressure head to apply pressure, maintaining the pressure for a certain period of time and then cooling to obtain a smart metal part with embedded sensors. The smart metal part with embedded sensors is prepared in one step while completing the metallurgical bonding of dissimilar metal materials, which has the following advantages:
[0023] (1) High sample precision and easy control of structural orientation. The additive manufacturing technology is used to prepare the TPMS structure porous rod frame. Compared with the traditional manufacturing process, the rod diameter and surface accuracy are higher. In terms of structural orientation, it can be arbitrarily controlled due to modeling in the computer, and the volume ratio of the strong and tough phase is highly operable.
[0024] (2) Save material costs and shorten the process flow. In the past, sensor packaging usually required two packaging steps, one at the primary level and the other at the secondary level, before being prepared into parts due to the fragility of fiber Bragg grating (FBG) sensors to ensure that the sensors were not damaged during operation. The present invention utilizes the high temperature resistance of high-temperature femtosecond metal-coated fiber Bragg grating (FBG) sensors and performs one-step packaging of sensors and bimetallic composites through quantitative extrusion casting, which saves material costs while solving the problem of complex fiber sensor packaging process.
[0025] (3) Good performance and stable life. The three-periodic minimal surface (TPMS) bionic structure in organisms is used to prepare a high-strength porous rod frame. Then, by taking advantage of the difference in the performance of the material components and imitating the strong and tough alternating arrangement of the nacre layer, a high-performance bionic interpenetrating material is prepared. The fiber Bragg grating (FBG) sensor has a stable service life when coated with this material. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0027] Figure 1 Schematic diagram of the process of the extrusion casting method according to an embodiment of the present invention.
[0028] Figure 2 This is a schematic diagram of the P structure of the TPMS type of the smart metal part with embedded sensor according to Example 1 of the present invention.
[0029] Figure 3This is a schematic diagram of the D structure of the TPMS type of the smart metal part with embedded sensor according to Example 2 of the present invention.
[0030] Figure 4 The density analysis of the smart metal part with embedded sensor of D structure prepared in Example 2 of the present invention.
[0031] 1-pressing head, 2-heating body, 3-porous rod frame, 4-aluminum alloy melt, 5-optical fiber sensor, 6-ejector, 7-intelligent metal part with embedded sensor.
[0032] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0033] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] According to one aspect of the present invention, the present invention provides the following technical solution:
[0035] like Figure 1 As shown, a method for extrusion casting of a smart metal part with an embedded sensor comprises the following steps:
[0036] S1, preparing a porous rod frame 3 having a TPMS bionic structure;
[0037] S2, selecting a preset structural health detection position for the porous rod frame 3, inserting the optical fiber sensor 5 into the preset structural health detection position, and placing it into the extrusion die;
[0038] S3, adding aluminum alloy melt 4 into the extrusion die, then controlling the pressure head 1 to apply pressure, maintaining the pressure for a certain period of time and then cooling, to obtain a smart metal part 7 with an embedded sensor.
[0039] Preferably, in step S1, the porous rod frame 3 is a porous titanium alloy rod frame or a porous stainless steel rod frame; the titanium alloy is Ti-6Al-4V titanium alloy, and the stainless steel is 316L stainless steel.
[0040] Preferably, in the step S1, a porous rod frame 3 having a TPMS bionic structure is prepared by an additive manufacturing process. The specific process is: using Matlab software to establish a three-dimensional model of a three-periodic minimal surface (TPMS) through implicit trigonometric functions, importing it into Materialise Magics 23.0, and setting the parameters of the TPMS structure. Subsequently, a new processing platform is created in MaterialiseMagics 23.0, and the parts are dragged onto the substrate for slicing. Secondly, the EPHatch software in the additive manufacturing equipment is opened, the slicing is saved, and the operation on the computer is completed; then, the equipment and machine interface are operated to set the additive manufacturing process parameters: for example, a scanning delay of 10μs, a jump delay of 50μs, a substrate temperature of 120°C, a filling laser power of 170~280W, a scanning speed of 600~1400mm / s, and a scanning spacing of 0.08mm. Finally, the powder bin is filled with alloy powder, and the protective gas is filled to perform additive manufacturing.
[0041] Preferably, in step S1, the porous rod frame 3 is placed in a NaOH solution with a concentration of 10-20wt% for alkaline washing for 5-10 minutes to remove oil stains on the surface of the porous rod frame 3, and then the porous rod frame 3 is placed in a hydrochloric acid solution with a concentration of 10-20wt% for pickling for 5-10 minutes to remove rust and other oxide layers of the porous rod frame 3, and finally cleaned with alcohol to achieve a cleanliness that meets casting requirements.
[0042] Preferably, in step S1, the cleaned porous titanium alloy rod frame is placed in a plating aid solution of 8.3wt% K2ZrF6-8.3wt% KCl-0.08wt% NaF at a temperature of 85-95°C for 5-10 minutes, taken out, and placed in an oven at 195-205°C for drying for 30 minutes to complete the plating aid treatment. The plating aid forms a salt film on the surface of the titanium alloy to prevent the titanium alloy from being exposed to air and being oxidized, and to maintain the surface activity of the porous titanium alloy rod frame.
[0043] Preferably, in step S1, the cleaned porous stainless steel rod frame is placed in a 6wt%KF-2wt%ZnCl2 plating aid solution at a temperature of 65-75°C for 15-20 minutes, taken out, and placed in an oven at 105-115°C for drying for 15 minutes to complete the plating aid treatment.
[0044] Preferably, in step S2, the selection of the health detection position must meet two points: first, surround and support the optical fiber sensor 5 to prevent damage to the optical fiber sensor 5 due to high pressure during extrusion casting; second, position the optical fiber sensor 5, fix the optical fiber sensor 5 using the TPMS structural units arranged in a regular periodic manner, and locate the position for sensor health detection.
[0045] Preferably, in step S2, the optical fiber sensor 5 is a high-temperature femtosecond metal-clad optical fiber Bragg grating sensor.
[0046] Preferably, in step S2, both ends of the optical fiber are left outside the mold to facilitate the collection of subsequent detection signals.
[0047] Preferably, in step S3, the extrusion die is preheated to prevent the aluminum alloy melt 4 from being quenched and damaging the bonding interface, and when the die temperature reaches 200-400°C, a preset weight of the aluminum alloy melt 4 is added to the extrusion die through an electromagnetic quantitative conveying device.
[0048] Preferably, in step S3, the pressure is 150-180 MPa, and the pressure is maintained for 30-60 seconds.
[0049] Preferably, in step S3, the aluminum alloy is an Al-Si alloy.
[0050] Preferably, in step S3, the smart metal part 7 with embedded sensors can obtain stress, strain and temperature values of the test part through feedback signals.
[0051] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0052] Example 1
[0053] This embodiment provides an extrusion casting method for a smart metal part with an embedded sensor, comprising the following steps:
[0054] S1. Prepare a porous rod frame 3 having a P structure of the TPMS type; the porous rod frame 3 is a porous titanium alloy rod frame; the titanium alloy is Ti-6Al-4V titanium alloy. A porous titanium alloy rod frame with a P structure in the TPMS type was prepared by an additive manufacturing process. The specific process was as follows: a three-dimensional model of a three-periodic minimal surface (TPMS) was established by using Matlab software through implicit trigonometric functions, and the model was imported into Materialise Magics 23.0. The parameters of the TPMS structure were set, and the smallest structural unit of P was set to 5mm*5mm*5mm, the thinnest rod diameter was set to 2mm, the adjacent units were close together without gaps, and the volume fraction of the porous titanium alloy rod frame in the overall smart metal part 7 with embedded sensors was 30%. Subsequently, a new processing platform was created in Materialise Magics 23.0, and the part was dragged onto the substrate for slicing. Secondly, the EPHatch software in the additive manufacturing equipment was opened, the slices were saved, and the operation on the computer was completed. After that, the equipment and machine interface were operated, and the additive manufacturing process parameters were set (as shown in Table 4). Finally, the powder bin was filled with Ti-6Al-4V titanium alloy powder (composition shown in Table 1), and the protective gas was filled for additive manufacturing. The porous titanium alloy rod frame is placed in a 10wt% NaOH solution for alkaline washing for 10 minutes to remove the oil stains on the surface of the porous titanium alloy rod frame, and then the porous titanium alloy rod frame is placed in a 10wt% hydrochloric acid solution for pickling for 10 minutes to remove the rust and other oxide layers of the porous titanium alloy rod frame, and finally cleaned with alcohol to achieve a cleanliness that meets the casting requirements. The cleaned porous titanium alloy rod frame is placed in a 8.3wt%K2ZrF6-8.3wt%KCl-0.08wt%NaF plating agent solution at a temperature of 95°C for 5 minutes, then taken out and placed in a 200°C oven for drying for 30 minutes to complete the plating agent treatment. The plating agent forms a salt film on the surface of the titanium alloy to prevent the titanium alloy from being exposed to the air and being oxidized, and maintain the surface activity of the porous titanium alloy rod frame.
[0055] S2. Select the preset structural health detection position for the porous titanium alloy rod frame, insert the optical fiber sensor 5 into the preset structural health detection position, and put it into the extrusion mold; the selection of the health detection position must meet two points: first, surround and support the optical fiber sensor 5 to prevent damage to the optical fiber sensor 5 by high pressure during extrusion casting; second, position the optical fiber sensor 5, fix the optical fiber sensor 5 using the regularly periodically arranged TPMS structural units, and locate the position of the sensor health detection. After combining the above two points, Example 1 inserts the optical fiber sensor 5 into the center line position of the P structural unit array. The two ends of the optical fiber are left outside the mold to facilitate the collection of subsequent detection signals.
[0056] S3, preheating the extrusion die, inserting the heating body 2 into the extrusion die, preheating the die, preventing the aluminum alloy melt 4 from being quenched and damaging the bonding interface, when the die temperature reaches 300°C, adding a preset weight of aluminum alloy melt 4 (composition see Table 2) into the extrusion die through electromagnetic quantitative conveying equipment, the current output value loaded on the electromagnetic pump electrode is 1400A, and the current intensity in the electromagnetic coil is 50A. At this time, the P-structure porous titanium alloy rod frame with the sensor embedded in the die is covered by the aluminum alloy melt, the pressure head 1 is lowered, and a pressure of 180MPa is applied, and the pressure is maintained for 35s. After the material is cooled, the pressure is removed, the pressure head 1 is raised, the cavity is opened, and the ejector 6 ejects the intelligent metal part 7 with the embedded sensor. The intelligent metal part can provide real-time signal feedback to the environment, and the stress, strain and temperature values of the assembly part can be measured through the feedback signal.
[0057] Example 2
[0058] This embodiment provides an extrusion casting method for a smart metal part with an embedded sensor, comprising the following steps:
[0059] S1. Prepare a porous rod frame 3 having a D structure in the TPMS type; the porous rod frame 3 is a porous titanium alloy rod frame; the titanium alloy is Ti-6Al-4V titanium alloy. A porous titanium alloy rod frame with a D structure in the TPMS type was prepared by an additive manufacturing process. The specific process was as follows: a three-dimensional model of a three-periodic minimal surface (TPMS) was established by using Matlab software through implicit trigonometric functions, and the model was imported into Materialise Magics 23.0. The parameters of the TPMS structure were set, and the smallest structural unit of D was set to 4mm*4mm*4mm, the thinnest rod diameter was set to 2mm, and the adjacent units were close to each other without gaps. The volume fraction of the porous titanium alloy rod frame in the overall smart metal part 7 with embedded sensors was 30%. Subsequently, a new processing platform was created in Materialise Magics 23.0, and the part was dragged onto the substrate for slicing. Secondly, the EPHatch software in the additive manufacturing equipment was opened, the slices were saved, and the operation on the computer was completed. After that, the equipment and machine interface were operated, and the additive manufacturing process parameters were set (as shown in Table 4). Finally, the powder bin was filled with Ti-6Al-4V titanium alloy powder (composition shown in Table 1), and the protective gas was filled for additive manufacturing. The porous titanium alloy rod frame is placed in a 10wt% NaOH solution for alkaline washing for 10 minutes to remove the oil stains on the surface of the porous titanium alloy rod frame, and then the porous titanium alloy rod frame is placed in a 10wt% hydrochloric acid solution for pickling for 10 minutes to remove the rust and other oxide layers of the porous titanium alloy rod frame, and finally cleaned with alcohol to achieve a cleanliness that meets the casting requirements. The cleaned porous titanium alloy rod frame is placed in a 8.3wt%K2ZrF6-8.3wt%KCl-0.08wt%NaF plating agent solution at a temperature of 85°C for 8 minutes, then taken out and placed in a 200°C oven for drying for 30 minutes to complete the plating agent treatment. The plating agent forms a salt film on the surface of the titanium alloy to prevent the titanium alloy from being exposed to the air and being oxidized, and maintain the surface activity of the porous titanium alloy rod frame.
[0060] S2. Select the preset structural health detection position for the porous titanium alloy rod frame, insert the optical fiber sensor 5 into the preset structural health detection position, and put it into the extrusion mold; the selection of the health detection position must meet two points: first, surround and support the optical fiber sensor 5 to prevent damage to the optical fiber sensor 5 by high pressure during extrusion casting; second, position the optical fiber sensor 5, fix the optical fiber sensor 5 using the regularly periodically arranged TPMS structural units, and locate the position of the sensor health detection. After combining the above two points, Example 2 inserts the optical fiber sensor 5 into the center line position of the D structural unit array. The two ends of the optical fiber are left outside the mold to facilitate the collection of subsequent detection signals.
[0061] S3. Preheat the extrusion die, insert the heating body 2 into the extrusion die, preheat the die to prevent the aluminum alloy melt 4 from being quenched and destroying the bonding interface. When the die temperature reaches 300°C, add a preset weight of aluminum alloy melt 4 (the composition is shown in Table 2) into the extrusion die through an electromagnetic quantitative conveying device. The current output value loaded on the electromagnetic pump electrode is 1400A, and the current intensity in the electromagnetic coil is 50A. At this time, the P-structured porous titanium alloy rod frame with the sensor embedded in the die is covered by the aluminum alloy melt. The pressure head 1 descends and applies a pressure of 150MPa for 60s. After the material cools down, the pressure is released, the pressure head 1 rises, the cavity is opened, and the ejector 6 ejects the smart metal part 7 with the embedded sensor. The smart metal part can provide real-time signal feedback to the environment, and the stress, strain and temperature values of the assembly part can be measured through the feedback signal. The density analysis of the smart metal part with embedded sensor of D structure prepared in Example 2 is as follows Figure 4 As shown by Figure 4 It can be seen that the internal structure of the smart metal part 7 with embedded sensors is tightly integrated, without defects such as cracks and unfilled parts, and the micropores are mainly concentrated in the titanium bracket.
[0062] Example 3
[0063] This embodiment provides an extrusion casting method for a smart metal part with an embedded sensor, comprising the following steps:
[0064] S1. Prepare a porous rod frame 3 having a D structure in the TPMS type; the porous rod frame is a porous stainless steel rod frame; the stainless steel is 316L stainless steel. A porous stainless steel rod frame with a P structure in the TPMS type was prepared by an additive manufacturing process. The specific process was as follows: a three-dimensional model of a three-periodic minimal surface (TPMS) was established by using Matlab software through implicit trigonometric functions, and the model was imported into Materialise Magics 23.0. The parameters of the TPMS structure were set, and the smallest structural unit of P was set to 4mm*4mm*4mm, the thinnest rod diameter was set to 2mm, and the adjacent units were close together without gaps. The volume fraction of the porous stainless steel rod frame in the overall smart metal part 7 with embedded sensors was 30%. Subsequently, a new processing platform was created in Materialise Magics 23.0, and the part was dragged onto the substrate for slicing. Secondly, the EPHatch software in the additive manufacturing equipment was opened, the slicing was saved, and the operation on the computer was completed. After that, the equipment and machine interface were operated, and the additive manufacturing process parameters were set (as shown in Table 4). Finally, 316L stainless steel powder (composition shown in Table 3) was filled into the powder bin, and protective gas was filled for additive manufacturing. The porous stainless steel rod frame was placed in a 10wt% NaOH solution for alkaline washing for 10 minutes to remove the oil stains on the surface of the porous stainless steel rod frame, and then the porous stainless steel rod frame was placed in a 10wt% hydrochloric acid solution for pickling for 10 minutes to remove the rust and other oxide layers of the porous stainless steel rod frame, and finally cleaned with alcohol to achieve a cleanliness that meets the casting requirements. The cleaned porous stainless steel rod frame was placed in a 6wt%KF-2wt%ZnCl2 plating agent solution at a temperature of 70°C for 15 minutes, then taken out and placed in a 110°C oven for drying for 15 minutes to complete the plating treatment.
[0065] S2. Select the preset structural health detection position for the porous stainless steel rod frame, insert the optical fiber sensor 5 into the preset structural health detection position, and put it into the extrusion mold; the selection of the health detection position must meet two points: first, surround and support the optical fiber sensor 5 to prevent damage to the optical fiber sensor 5 by high pressure during extrusion casting; second, position the optical fiber sensor 5, fix the optical fiber sensor 5 using the regularly periodically arranged TPMS structural units, and locate the position of the sensor health detection. After combining the above two points, Example 3 inserts the optical fiber sensor 5 into the center line position of the P structural unit array. The two ends of the optical fiber are left outside the mold to facilitate the collection of subsequent detection signals.
[0066] S3, preheating the extrusion die, inserting the heating body 2 into the extrusion die, preheating the die, preventing the aluminum alloy melt 4 from being quenched and damaging the bonding interface, when the die temperature reaches 300°C, adding a preset weight of aluminum alloy melt 4 (composition see Table 2) into the extrusion die through electromagnetic quantitative conveying equipment, the current output value loaded on the electromagnetic pump electrode is 1400A, and the current intensity in the electromagnetic coil is 50A. At this time, the P-structured porous stainless steel rod frame with the sensor embedded in the die is covered by the aluminum alloy melt, the pressure head 1 descends, and a pressure of 150MPa is applied, and the pressure is maintained for 60s. After the material cools, the pressure is removed, the pressure head 1 rises, the cavity is opened, and the ejector 6 ejects the intelligent metal part 7 with the embedded sensor. The intelligent metal part can provide real-time signal feedback to the environment, and the stress, strain and temperature values of the assembly part can be measured through the feedback signal.
[0067] Table 1 Chemical composition of titanium alloy (wt%)
[0068]
[0069] Table 2 Chemical composition of aluminum alloy (wt%)
[0070]
[0071] Table 3 Chemical composition of stainless steel (wt%)
[0072]
[0073] Table 4 Additive manufacturing process parameters
[0074]
[0075] The present invention prepares a porous rod frame with a TPMS bionic structure; selects a preset structural health detection position for the porous rod frame, inserts an optical fiber sensor into the preset structural health detection position, and puts it into an extrusion die; adds aluminum alloy melt to the extrusion die, then controls the pressure head to apply pressure, maintains the pressure for a certain period of time, and then cools to obtain an intelligent metal part with an embedded sensor. While completing the metallurgical bonding of dissimilar metal materials, an intelligent metal part with an embedded sensor is prepared in one step, and the bionic structure and component composition are used to give full play to the physical properties of the dissimilar metal materials, ensuring that the coated FBG sensor is not damaged.
[0076] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. An extrusion casting method for smart metal parts with embedded sensors, It is characterized in that The steps include: S1. Prepare a porous rod frame with a TPMS bionic structure. Prepare a porous rod frame with a TPMS bionic structure by additive manufacturing. The specific process is as follows: Use Matlab software to establish a 3D model of TPMS through implicit trigonometric functions, import it into Materialise Magics 23.0, set the parameters of the TPMS structure, and then Create a new processing platform in Magics23.0, drag the parts to the substrate, and slice them. Then, open the EPHatch software in the additive manufacturing equipment, save the slices, and complete the operation on the computer. Then operate the equipment and machine interface, set the additive manufacturing process parameters, and finally fill the powder bin with alloy powder and protective gas for additive manufacturing. Put the porous rod frame into a NaOH solution with a concentration of 10~20wt% for alkaline washing for 5~10min, then put the porous rod frame into a hydrochloric acid solution with a concentration of 10~20wt% for pickling for 5~10min, and finally clean it with alcohol. Put the cleaned porous titanium alloy rod frame into an 8.3wt%K 2 ZF 6 -8.3wt%KCl-0.08wt%NaF plating agent solution for 5-10 minutes, then take it out and put it in a 195-205℃ oven for drying for 30 minutes to complete the plating treatment or put the cleaned porous stainless steel rod rack into 6wt%KF-2wt%ZnCl at a temperature of 65-75℃ 2 After 15-20 minutes in the plating agent solution, take it out and put it in a 105-115℃ oven for drying for 15 minutes to complete the plating agent treatment; S2. Selecting a preset structural health detection position for the porous rod frame, inserting the optical fiber sensor into the preset structural health detection position, and placing it into the extrusion die; The selection of the health detection position must meet two points: first, surround and support the optical fiber sensor to prevent damage to the optical fiber sensor by high pressure during extrusion casting; second, position the optical fiber sensor, fix the optical fiber sensor using the regularly periodically arranged TPMS structural units, and locate the position of the sensor health detection; the optical fiber sensor is a high-temperature femtosecond metal-coated fiber Bragg grating sensor; S3. Add aluminum alloy melt into the extrusion die, then control the pressure head to apply pressure, maintain the pressure for a certain period of time and then cool it down. The pressure is 150-180 MPa, and the pressure is maintained for 30-60 seconds to obtain a smart metal part with an embedded sensor.
2. The extrusion casting method of the smart metal part with embedded sensor according to claim 1, It is characterized in that In the step S1, the porous rod frame is a porous titanium alloy rod frame or a porous stainless steel rod frame; the titanium alloy is Ti-6Al-4V titanium alloy, and the stainless steel is 316L stainless steel.
3. The extrusion casting method of the smart metal part with embedded sensor according to claim 1, It is characterized in that In the step S3, the extrusion die is preheated, and when the die temperature reaches 200-400° C., a preset weight of aluminum alloy melt is added into the extrusion die through an electromagnetic quantitative conveying device; the aluminum alloy is an Al-Si alloy.
Citation Information
Patent Citations
Porous magnesium alloy / biological ceramic bionic composite support and quick forming method thereof
CN102327648A
Method for manufacturing Al-Sn alloy-based nickel-plated high-temperature-resistant fiber grating sensor
CN102601344A
Package structure for composite sensor module and manufacturing method of package structure
CN105609490A
Self-sensing dual-cavity multi-freedom-degree pneumatic flexible bionic finger
CN107214696A
Bimetal composite casting method for cylinder cover of automobile engine cylinder
CN107790681A