Antibacterial polyester and its preparation method and application
The alcohol-based rare earth functional dispersion liquid was introduced into the antibacterial polyester through in situ polymerization, which solved the problem of uneven dispersion and insufficient stability of the antibacterial polyester material during the preparation process, and achieved excellent antibacterial performance and environmental friendliness for common bacteria efficient sterilization effect.
Patent Information
- Application Number
- CN202411178946.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-27
AI Technical Summary
During the preparation process, existing antibacterial polyester materials have problems with solvent recovery, uneven dispersion of antibacterial components, poor compatibility and insufficient stability, and are insufficient for environmental pollution and bacterial durability.
In-situ polymerization method is used to dopate the alcohol-based rare earth functional dispersion into the polymer matrix, and through multi-stage grinding and chemical bonding, a stable alcohol-based rare earth functional dispersion is formed, improving the antibacterial properties and stability of the antibacterial polyester.
It has achieved excellent antibacterial properties against common bacteria such as E. coli and Staphylococcus aureus. It is insoluble in antibacterial components, safe and environmentally friendly, and is suitable for antibacterial fibers, medical mattresses and packaging films.
Smart Images

Figure CN118702904B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a novel antibacterial polyester and a preparation method and application thereof. Background Art
[0002] The preparation methods of antibacterial polyester are mainly surface treatment, post-finishing, blending modification, in-situ polymerization, etc. Surface treatment and post-finishing methods are relatively economical and simple, but the molecules are combined by van der Waals force and electrostatic action, the binding force is weak, the durability is poor, and the antibacterial component may also cause certain pollution to the environment as it falls off. Blending modification is easy to mass produce, easy to operate, and the antibacterial agent can be added flexibly. It is commonly used in industry, but there is a problem of solvent recovery in solution blending, which may cause environmental pollution. Melt blending is relatively environmentally friendly, but the dispersion of antibacterial components in the matrix mainly depends on the mechanical shear force provided by the mixing equipment. The antibacterial components cannot be evenly dispersed, have poor compatibility with the matrix, and are prone to agglomeration and precipitation, resulting in poor stability of the polymer. In-situ polymerization is to fully mix the antibacterial component with the polymer monomer (including a monomer or a blend of multiple monomers) or prepolymer to produce a polymerization reaction. In-situ polymerization has a good dispersion effect, is not easy to agglomerate, has a strong binding force between the antibacterial component and the matrix, does not dissolve, and has strong antibacterial durability.
[0003] Rare earth is a general term for 17 metal elements in the periodic table, including lanthanide elements, scandium and yttrium. There are 250 kinds of rare earth ores in nature. China's rare earth resources are not only rich in reserves, but also have the advantages of complete mineral species and rare earth elements, reasonable distribution of rare earth grades and mineral points. Rare earth is known as the "gold" of industry. It can be combined with other materials to form new materials with different properties and a wide variety. Its most significant function is to greatly improve the quality and performance of other products. Through research, it is found that after rare earth functional materials react completely with COOH, C=O on peptidoglycan in bacteria or P=O, P-O- in teichoic acid, the conformation is completely changed, a pathway is formed, and the cell contents are extravasated. A large number of rare earth ions enter the cell and interact with biological molecules such as DNA, enzymes, and proteins in the cell, hindering normal physiological metabolism, thereby inhibiting the growth of bacteria until it stops completely.
[0004] Therefore, if rare earth ions are applied to polyester, polyester materials with better antibacterial effects will be obtained. Summary of the invention
[0005] In view of this, the present invention aims to propose a novel antibacterial polyester and its preparation method and application, wherein an alcohol-based rare earth functional dispersion is doped into a polymer matrix by an in-situ polymerization method, and the addition of rare earth functional components greatly improves the antibacterial properties of the polyester, and exhibits excellent antibacterial properties against common Gram-negative and Gram-positive bacteria such as Escherichia coli (E.coli) and Staphylococcus aureus (S.aureus). The antibacterial components of the polyester have strong binding force and good compatibility with the polymer matrix, have little effect on the mechanical properties of the polymer, are highly effective in sterilization without dissolution, are safe and environmentally friendly, and can be applied to the fields of antibacterial fibers, medical mattresses, packaging films, etc.
[0006] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0007] A method for preparing a novel antibacterial polyester, the method comprising the following steps:
[0008] 1) Preparation of rare earth functional powders:
[0009] Putting nitrogen-containing compounds, guanidine hydrochloride, rare earth chloride and deionized water into a reaction kettle and stirring them evenly; then adding concentrated sulfuric acid into the reaction kettle to react and obtain an intermediate product; putting the intermediate product into an oven to dry, grinding the dried intermediate product, and then putting it into a muffle furnace to calcine it;
[0010] 2) Preparation of alcohol-based rare earth functional dispersion:
[0011] The rare earth functional powder obtained in step 1) and the aliphatic diol are mixed evenly, and added to a sand mill for thorough grinding; then a dispersant is added, and multi-stage grinding is performed in a sand mill to obtain a uniformly dispersed alcohol-based rare earth functional dispersion;
[0012] 3) Preparation of antibacterial polyester:
[0013] The alcohol-based rare earth functional dispersion, aliphatic diol, dibasic acid, stabilizer and catalyst are weighed by mass to prepare a polymerization slurry, which is then put into a high-pressure reactor for esterification and polycondensation to obtain a rare earth functional polyester melt; the obtained rare earth functional polyester melt is cooled and pelletized, and transported to a solid phase viscosity increasing system for crystallization and solid phase polycondensation to obtain a novel antibacterial polyester chip.
[0014] Before the polymerization reaction, the corresponding dispersant is added to fully and evenly mix the rare earth functional powder and the polymerization monomer (aliphatic diol). The rare earth functional component and the aliphatic diol are tightly combined together through chemical bonds or intermolecular forces to form a stable alcohol-based rare earth functional dispersion. After the alcohol-based rare earth functional dispersion is added to the polymerization reaction, when the aliphatic diol and the dibasic acid undergo esterification and condensation reactions, the rare earth functional component can be better and more evenly grafted into the polyester molecular chain to obtain a functional polyester uniformly doped with rare earths.
[0015] If rare earth functional powder is directly added to the polymerization reaction, the nanomaterial may partially agglomerate due to its smaller particle size and cannot participate in the polymerization reaction stably and evenly. The functional components in the obtained polyester are unevenly distributed and the stability of the back-end application is poor.
[0016] Furthermore, the rare earth functional powder includes 5-30 parts of nitrogen-containing compounds, 15-80 parts of guanidine hydrochloride, 35-65 parts of rare earth chloride, and 50-200 parts of deionized water by weight; 3-25 mL of concentrated sulfuric acid is added;
[0017] The nitrogen-containing compound is a mixture of melamine, dicyandiamide and urea, wherein the molar ratio of melamine, dicyandiamide and urea is 1-3:6-8:1.
[0018] The rare earth chloride is a mixture of lanthanum chloride and one of cerium chloride, yttrium chloride or gadolinium chloride, and the molar ratio of lanthanum chloride to cerium chloride / yttrium chloride / gadolinium chloride is 3-5:1-2.
[0019] Furthermore, in step 1), the temperature of the reactor is 70-150° C., and the stirring is performed for 3-8 hours; the drying temperature is 100-200° C.; and the calcination temperature is 300-1000° C., and the time is 2-7 hours.
[0020] Furthermore, the alcohol-based rare earth functional dispersion comprises 20-35 parts of rare earth functional powder, 60-79 parts of aliphatic diol, and 1-5 parts of dispersant by weight; the particle size of the alcohol-based rare earth functional dispersion is 100-300nm; the dispersant is a mixture of one or more of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate, modified styrene maleic acid copolymer solution, modified polymer block copolymer, and high molecular weight silane copolymer containing pigment-affinity groups.
[0021] Furthermore, in step 3), the esterification reaction temperature is 220-300°C, the polycondensation reaction temperature is 240-300°C, the crystallization temperature is 130-190°C, and the solid phase polycondensation reaction temperature is 180-220°C.
[0022] Furthermore, the aliphatic diol in step 2) and step 3) is the same substance, and the aliphatic diol is any one of ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol and decanediol. The aliphatic diol is the same substance to ensure good compatibility between the dispersion and the polymerization slurry, which is beneficial to the uniform dispersion of the rare earth functional powder in the polymerization slurry and is more conducive to the stability of the polymerization reaction.
[0023] Further, in step 3), the dibasic acid is a mixture of one or two of terephthalic acid, isophthalic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid and sebacic acid;
[0024] The stabilizer is a mixture of one or more of trimethyl phosphite, trimethyl phosphate, triphenyl phosphate, triethyl phosphate, and bis(2,4-dicumylphenyl)pentaerythritol-diphosphite;
[0025] The catalyst is a mixture of one or more antimony catalysts, titanium catalysts, and germanium catalysts. The antimony catalyst is one or more of ethylene glycol antimony, antimony trioxide, or antimony acetate. The titanium catalyst is one or more of tetrabutyl titanate, ethylene glycol titanium, tetraisopropyl titanate, Ti / Zn catalyst, and titanic acid. The germanium catalyst is germanium dioxide.
[0026] Furthermore, in step 3), the molar ratio of the dibasic acid to the aliphatic diol is 1:1.1-1.7, the mass of the stabilizer is 0.003-0.05% of the total mass of the polymerization slurry, the mass of the catalyst is 0.02-0.15% of the total mass of the polymerization slurry, and the rare earth functional powder accounts for 0.5%-5% of the total mass of the polymerization slurry.
[0027] The present invention also provides a novel antibacterial polyester prepared by any of the above-mentioned preparation methods.
[0028] The present invention also provides an application of the new antibacterial polyester as described above in antibacterial functional fibers, medical mattresses, and packaging films. The characteristic viscosity of the new polyester chips is 0.6-1.4dL / g, and the new antibacterial polyester chips are made into corresponding fibers, plastics, and films for application.
[0029] Compared with the prior art, the novel antibacterial polyester and its preparation method and application described in the present invention have the following advantages:
[0030] 1. The rare earth functional powder of the present invention is prepared by a series of chemical reactions and high-temperature calcination. It is a rare earth-doped carbon nitride nanomaterial. This composite material acts on the surface of bacteria through the synergistic effect of rare earth and carbon nitride nanomaterials, changes the cell structure, interacts with biological molecules such as DNA, enzymes, and proteins in the cells, hinders the normal physiological metabolism of bacteria, thereby inhibiting the growth of bacteria until it stops completely, giving the material excellent antibacterial properties.
[0031] 2. Through multi-stage grinding, the rare earth functional powder and the polymerization monomer are fully mixed before polymerization, so that the rare earth antibacterial functional powder is highly evenly dispersed in the polymerization system, which is convenient for participating in the polymerization reaction, improves the stability of polymerization production, and ensures the stability of downstream applications.
[0032] 3. The alcohol-based rare earth functional dispersion is introduced into the polyester production through the in-situ polymerization method, which enhances the binding force and compatibility between the antibacterial component and the matrix, ensures the stability and uniformity of the rare earth functional polyester chip structure, the antibacterial component is added in a low amount and does not dissolve, and has strong antibacterial durability.
[0033] 4. The obtained new antibacterial polyester chips show excellent antibacterial properties against common Gram-negative bacteria and Gram-positive bacteria such as Escherichia coli (E. coli) and Staphylococcus aureus (S. aureus), with high efficiency in sterilization without dissolution, safety and environmental protection, and can be applied to antibacterial functional fibers, medical mattresses, packaging films and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0035] Figure 1 This is a flow chart for the preparation of new antibacterial polyester. DETAILED DESCRIPTION
[0036] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Example 1
[0039] A method for preparing a novel antibacterial polyester, the method comprising the following steps:
[0040] 1) Preparation of rare earth functional powders:
[0041] Weigh 10 parts of nitrogen-containing compounds (wherein the molar ratio of melamine, dicyandiamide and urea is 3:6:1), 30 parts of guanidine hydrochloride, 35 parts of rare earth chlorides (wherein the molar ratio of lanthanum chloride and cerium chloride is 3:1), and 100 parts of deionized water by mass and put them into a reactor, and stir them evenly; then add 10 mL of concentrated sulfuric acid into the reactor, set the temperature of the reactor to 70°C, stir for 5 hours, and obtain an intermediate product; put the intermediate product into an oven and dry it at 150°C, grind the dried intermediate product, put it into a muffle furnace and calcine it at 400°C for 5 hours, and obtain a rare earth functional powder.
[0042] 2) Preparation of alcohol-based rare earth functional dispersion:
[0043] Weigh 23 parts of rare earth functional powder and 76 parts of ethylene glycol by mass, mix them evenly, add them to a sand mill and grind them for 2 hours; then add 1 part of dispersant polyvinyl pyrrolidone, grind them in a sand mill for 6 hours in multiple stages to disperse them evenly, and obtain an alcohol-based rare earth functional dispersion with a particle size of 146 nm.
[0044] 3) Preparation of new antibacterial polyester:
[0045] The alcohol-based rare earth functional dispersion, ethylene glycol, terephthalic acid, stabilizer trimethyl phosphate and catalyst ethylene glycol antimony are weighed by mass to prepare a polymerization slurry, which is put into a high-pressure reactor for esterification and polycondensation to obtain a rare earth functional polyester melt, wherein the esterification reaction temperature is 250°C and the polycondensation reaction temperature is 280°C; the melt is cooled and pelletized, and the slices are transported to a solid phase viscosity increasing system for crystallization and solid phase polycondensation reaction, wherein the crystallization temperature is 140°C and the solid phase polycondensation reaction temperature is 200°C, to obtain a new antibacterial polyester slice with a characteristic viscosity of 0.95dL / g.
[0046] The molar ratio of terephthalic acid and ethylene glycol in the slurry is 1:1.3, the mass of the stabilizer trimethyl phosphate is 0.02% of the total mass of the slurry, the mass of the catalyst ethylene glycol antimony is 0.05% of the total mass of the slurry, and the mass proportion of rare earth functional powder in the slurry is 2%.
[0047] 4) The dried new antibacterial polyester chips are added to the screw extruder, melted and extruded at high temperature by the screw to form a rare earth functional polyester melt, which is metered by a metering pump and enters the channel of the spinneret. The melt is extruded through the spinneret holes, cooled, oiled, stretched and wound to obtain the new antibacterial polyester fiber.
[0048] After testing, the antibacterial rates of Escherichia coli, Staphylococcus aureus and Candida albicans were >99%, >99% and >99%, respectively. After 50 washes, the antibacterial rates of Escherichia coli, Staphylococcus aureus and Candida albicans were 96%, >99% and >99%, respectively.
[0049] Example 2
[0050] A method for preparing a novel antibacterial polyester, the method comprising the following steps:
[0051] 1) Preparation of rare earth functional powders:
[0052] Weigh 20 parts of nitrogen-containing compounds (wherein the molar ratio of melamine, dicyandiamide and urea is 2:7:1), 50 parts of guanidine hydrochloride, 40 parts of rare earth chloride (wherein the molar ratio of lanthanum chloride and yttrium chloride is 5:2), and 120 parts of deionized water by mass, put them into a reactor, and stir them evenly; then add 15 mL of concentrated sulfuric acid into the reactor, set the temperature of the reactor to 90° C., stir for 6 hours, and obtain an intermediate product; put the intermediate product into an oven and dry it at 150° C.; grind the dried intermediate product and put it into a muffle furnace and calcine it at 500° C. for 5 hours to obtain a rare earth functional powder.
[0053] 2) Preparation of alcohol-based rare earth functional dispersion:
[0054] Weigh 28 parts of rare earth functional powder and 70 parts of pentanediol by mass, mix them thoroughly, add them to a sand mill and grind them thoroughly for 3 hours; then add 2 parts of dispersant-modified styrene maleic acid copolymer solution, perform multi-stage grinding in a sand mill for 5 hours to disperse them uniformly, and obtain an alcohol-based rare earth functional dispersion with a particle size of 175 nm.
[0055] 3) Preparation of new antibacterial polyester:
[0056] An alcohol-based rare earth functional dispersion, pentanediol, adipic acid, stabilizer triphenyl phosphate and a Ti / Zn catalyst are weighed by mass to prepare a polymerization slurry, which is put into a high-pressure reactor for esterification and polycondensation to obtain a rare earth functional polyester melt, wherein the esterification reaction temperature is 255°C and the polycondensation reaction temperature is 285°C; the melt is cooled and pelletized, and the slices are transported to a solid phase viscosity increasing system for crystallization and solid phase polycondensation reaction, wherein the crystallization temperature is 150°C and the solid phase polycondensation reaction temperature is 190°C, to obtain a new antibacterial polyester slice with a characteristic viscosity of 0.73dL / g.
[0057] The molar ratio of adipic acid to pentanediol in the slurry is 1:1.4, the mass of the stabilizer triphenyl phosphate is 0.04% of the total mass of the slurry, the mass of the catalyst Ti / Zn is 0.06% of the total mass of the slurry, and the mass of the rare earth functional powder in the slurry accounts for 3%.
[0058] 4) The dried new antibacterial polyester slices are injection molded, and the obtained engineering plastics have an antibacterial rate of >99% against Escherichia coli, >99% against Staphylococcus aureus, and >99% against Candida albicans.
[0059] Example 3
[0060] A method for preparing a novel antibacterial polyester, the method comprising the following steps:
[0061] 1) Preparation of rare earth functional powders:
[0062] Weigh 6 parts of nitrogen-containing compounds (wherein the molar ratio of melamine, dicyandiamide and urea is 1:8:1), 15 parts of guanidine hydrochloride, 55 parts of rare earth chloride (wherein the molar ratio of lanthanum chloride and gadolinium chloride is 4:1), and 180 parts of deionized water by mass and put them into a reactor, and stir them evenly; then add 10 mL of concentrated sulfuric acid into the reactor, set the temperature of the reactor to 110° C., stir for 8 hours, and obtain an intermediate product; put the intermediate product into an oven and dry it at 180° C., grind the dried intermediate product, put it into a muffle furnace and calcine it at 700° C. for 4 hours, and obtain a rare earth functional powder.
[0063] 2) Preparation of alcohol-based rare earth functional dispersion:
[0064] Weigh 34 parts of rare earth functional powder and 63 parts of butanediol by mass, mix them thoroughly, add them to a sand mill and grind them thoroughly for 4 hours; then add 3 parts of dispersant-modified polymer block copolymer, perform multi-stage grinding in a sand mill for 8 hours to disperse them uniformly, and obtain an alcohol-based rare earth functional dispersion with a particle size of 231 nm.
[0065] 3) Preparation of new antibacterial polyester:
[0066] Alcohol-based rare earth functional dispersion, butanediol, sebacic acid, stabilizer triethyl phosphate and catalyst germanium dioxide are weighed by mass to prepare a polymerization slurry, which is put into a high-pressure reactor for esterification and polycondensation to obtain a rare earth functional polyester melt, wherein the esterification reaction temperature is 245°C, and the polycondensation reaction temperature is 290°C; the melt is cooled and pelletized, and the slices are transported to a solid phase viscosity increasing system for crystallization and solid phase polycondensation reaction, wherein the crystallization temperature is 170°C, and the solid phase polycondensation reaction temperature is 220°C, to obtain a new antibacterial polyester slice with a characteristic viscosity of 1.20 dL / g.
[0067] The molar ratio of sebacic acid to butanediol in the slurry is 1:1.6, the mass of the stabilizer triethyl phosphate is 0.05% of the total mass of the slurry, the mass of the catalyst germanium dioxide is 0.09% of the total mass of the slurry, and the mass proportion of the rare earth functional powder in the slurry is 1%.
[0068] 4) The dried new antibacterial polyester slices were made into biaxially oriented polyester films, and the antibacterial rates against Escherichia coli, Staphylococcus aureus, and Candida albicans were 98%, >99%, >99%, and >99% respectively.
[0069] Comparative Example 1
[0070] The antibacterial properties of polyethylene terephthalate fiber without adding any functional components were tested, and the antibacterial rate against Escherichia coli was 0%, the antibacterial rate against Staphylococcus aureus was 0%, and the antibacterial rate against Candida albicans was 0%.
[0071] The results show that the novel antibacterial polyester prepared by the present invention exhibits excellent antibacterial properties against common Gram-negative bacteria and Gram-positive bacteria, the antibacterial component does not dissolve, and the antibacterial durability is strong.
[0072] Comparative Example 2
[0073] (1) Weigh 10 parts by weight of the rare earth functional powder prepared in Example 1 and 90 parts of polyethylene terephthalate powder and put them into a high-speed mixer and mix them at high and low speeds to mix them evenly. Use a melt blending method to put the mixed materials into a twin-screw granulator for blending, melt extrusion, and the twin-screw granulator has a speed of 300 r / min and a melting temperature of 260°C. After cooling and solidification, pelletize and dry to obtain a 10% rare earth functional polyester masterbatch.
[0074] (2) 20 parts of rare earth functional polyester masterbatch and 80 parts of polyethylene terephthalate chips after drying are added to the screw extruder, melted and extruded by the screw at high temperature to form a melt, which is metered by a metering pump and enters the channel of the spinneret. It is extruded through the spinneret hole, cooled, oiled, stretched, and wound to obtain fibers. According to the test, the antibacterial rate against Escherichia coli is 91%, the antibacterial rate against Staphylococcus aureus is 93%, and the antibacterial rate against Candida albicans is 88%.
[0075] After 50 times of washing, the antibacterial rate against Escherichia coli was 82%, the antibacterial rate against Staphylococcus aureus was 83%, and the antibacterial rate against Candida albicans was 80%.
[0076] Compared with Example 1, it is found that compared with the in-situ polymerization preparation process, the rare earth antibacterial polyester prepared by the masterbatch blending method has a weaker binding force with the matrix, reduced antibacterial performance, poor stability, and poor water washing resistance. After repeated water washing, the antibacterial rate decreases significantly.
[0077] Comparative Example 3
[0078] (1) The preparation of rare earth functional powder is the same as that in Example 1.
[0079] (2) The rare earth functional powder is directly added to the polymerization reactor without preparing an alcohol-based rare earth functional dispersion. Other steps are the same as in Example 1.
[0080] The spinning test revealed that the polyester chips had poor spinnability, unstable component pressure, easy blockage of the spinneret holes, easy breakage, and low yield.
[0081] This indicates that when the rare earth functional powder is directly added to the polymerization reactor instead of being added in the form of a dispersion, the rare earth functional powder may be partially agglomerated during the polymerization reaction and fail to participate well in the polymerization reaction, resulting in uneven polyester chips and poor spinnability.
[0082] Comparative Example 4
[0083] (1) Weigh 10 parts by mass of a nitrogen-containing compound (wherein the molar ratio of dicyandiamide to urea is 6:1), 30 parts by mass of guanidine hydrochloride, 35 parts by mass of a rare earth chloride (wherein the molar ratio of lanthanum chloride to cerium chloride is 3:1), and 100 parts by mass of deionized water, put them into a reactor, and stir them thoroughly; then add 10 mL of concentrated sulfuric acid into the reactor, set the reactor temperature to 70°C, stir for 5 hours, and obtain an intermediate product; put the intermediate product into an oven at 150°C and dry it; grind the dried intermediate product and put it into a muffle furnace and calcine it at 400°C for 5 hours to obtain a rare earth functional powder.
[0084] (2) Other conditions are the same as those in Example 1. The obtained fiber was tested, and the antibacterial rates against Escherichia coli, Staphylococcus aureus, and Candida albicans were 86%, 85%, and 82%, respectively.
[0085] Comparative Example 5
[0086] (1) Weigh 10 parts by mass of a nitrogen-containing compound (wherein the molar ratio of melamine to urea is 3:1), 30 parts by mass of guanidine hydrochloride, 35 parts by mass of a rare earth chloride (wherein the molar ratio of lanthanum chloride to cerium chloride is 3:1), and 100 parts by mass of deionized water, put them into a reactor, and stir them thoroughly; then add 10 mL of concentrated sulfuric acid into the reactor, set the reactor temperature to 70°C, stir for 5 hours, and obtain an intermediate product; put the intermediate product into an oven and dry it at 150°C, grind the dried intermediate product, put it into a muffle furnace, and calcine it at 400°C for 5 hours to obtain a rare earth functional powder.
[0087] (2) Other conditions are the same as those in Example 1. The obtained fiber was tested, and the antibacterial rates against Escherichia coli, Staphylococcus aureus, and Candida albicans were 84%, 87%, and 83%, respectively.
[0088] Comparative Example 6
[0089] (1) Weigh 10 parts by mass of a nitrogen-containing compound (wherein the molar ratio of melamine to dicyandiamide is 3:6), 30 parts by mass of guanidine hydrochloride, 35 parts by mass of a rare earth chloride (wherein the molar ratio of lanthanum chloride to cerium chloride is 3:1), and 100 parts by mass of deionized water, and put them into a reactor, and stir them thoroughly; then add 10 mL of concentrated sulfuric acid into the reactor, set the reactor temperature to 70°C, and stir for 5 hours to obtain an intermediate product; put the intermediate product into an oven to dry at 150°C, grind the dried intermediate product, and then put it into a muffle furnace to calcine at 400°C for 5 hours to obtain a rare earth functional powder.
[0090] (2) Other conditions are the same as those in Example 1. The obtained fiber was tested and its antibacterial rate against Escherichia coli was 89%, the antibacterial rate against Staphylococcus aureus was 91%, and the antibacterial rate against Candida albicans was 87%.
[0091] Comparative Example 7
[0092] (1) Weigh 10 parts by mass of nitrogen-containing compounds (wherein the molar ratio of melamine, dicyandiamide and urea is 2:2:3), 30 parts by mass of guanidine hydrochloride, 35 parts by mass of rare earth chloride (wherein the molar ratio of lanthanum chloride and cerium chloride is 3:1), and 100 parts by mass of deionized water, put them into a reactor, and stir them thoroughly; then add 10 mL of concentrated sulfuric acid into the reactor, set the reactor temperature to 70°C, stir for 5 hours, and obtain an intermediate product; put the intermediate product into an oven at 150°C and dry it, grind the dried intermediate product, put it into a muffle furnace and calcine it at 400°C for 5 hours, and obtain a rare earth functional powder.
[0093] (2) Other conditions are the same as those in Example 1. The obtained fiber was tested and its antibacterial rate against Escherichia coli was 85%, the antibacterial rate against Staphylococcus aureus was 86%, and the antibacterial rate against Candida albicans was 82%.
[0094] The results of comparative examples 4-7 show that when preparing rare earth functional powders, changing the composition and molar ratio of nitrogen-containing compounds will significantly reduce the antibacterial properties of the back-end products. The three components are indispensable and the molar ratio of the three cannot exceed the range.
[0095] Comparative Example 8
[0096] (1) Weigh 10 parts by mass of a melamine nitrogen-containing compound (wherein the molar ratio of melamine, dicyandiamide and urea is 3:6:1), 30 parts by mass of guanidine hydrochloride, 35 parts by mass of a rare earth chloride (all lanthanum chloride) and 100 parts by mass of deionized water, put them into a reactor and stir them thoroughly; then add 10 mL of concentrated sulfuric acid into the reactor, set the reactor temperature to 70°C, stir for 5 hours to obtain an intermediate product; put the intermediate product into an oven to dry at 150°C, grind the dried intermediate product and put it into a muffle furnace to calcine at 400°C for 5 hours to obtain a rare earth functional powder.
[0097] (2) Other conditions are the same as those in Example 1. The obtained fiber was tested and its antibacterial rate against Escherichia coli was 89%, the antibacterial rate against Staphylococcus aureus was 91%, and the antibacterial rate against Candida albicans was 89%.
[0098] Comparative Example 9
[0099] (1) Weigh 10 parts by mass of a melamine nitrogen-containing compound (wherein the molar ratio of melamine, dicyandiamide and urea is 3:6:1), 30 parts by mass of guanidine hydrochloride, 35 parts by mass of a rare earth chloride (wherein the molar ratio of lanthanum chloride and cerium chloride is 1:1), and 100 parts by mass of deionized water, put them into a reactor, and stir them thoroughly; then add 10 mL of concentrated sulfuric acid into the reactor, set the reactor temperature to 70°C, stir for 5 hours, and obtain an intermediate product; put the intermediate product into an oven at 150°C and dry it, grind the dried intermediate product, put it into a muffle furnace and calcine it at 400°C for 5 hours, and obtain a rare earth functional powder.
[0100] (2) Other conditions are the same as those in Example 1. The obtained fiber was tested and its antibacterial rate against Escherichia coli was 91%, that against Staphylococcus aureus was 93%, and that against Candida albicans was 90%.
[0101] The results of Comparative Examples 8 and 9 show that when preparing rare earth functional powders, changing the composition and molar ratio of rare earth chlorides will significantly reduce the antibacterial properties of the back-end products. The rare earth chlorides are mainly lanthanum chloride, and other rare earth chlorides are supplementary. Multiple rare earth elements work together to improve the antibacterial properties of the material through synergistic effects.
[0102] Comparative Example 10
[0103] 35 parts of rare earth fluoride (the molar ratio of lanthanum fluoride to cerium fluoride is 3:1), and the rest is the same as in Example 1.
[0104] The obtained fiber was tested and its antibacterial rate against Escherichia coli was 89%, the antibacterial rate against Staphylococcus aureus was 90%, and the antibacterial rate against Candida albicans was 75%.
[0105] Comparative Example 11
[0106] 35 parts of rare earth bromide (wherein the molar ratio of lanthanum bromide to cerium bromide is 3:1), and the rest is the same as in Example 1.
[0107] The obtained fiber was tested and the antibacterial rate against Escherichia coli was 87%, the antibacterial rate against Staphylococcus aureus was 96%, and the antibacterial rate against Candida albicans was 87%.
[0108] The results of Comparative Examples 10 and 11 show that compared with rare earth fluorides and rare earth bromides, rare earth chlorides have higher reactivity and improve the antibacterial properties of rare earth functional powders in fibers.
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an antibacterial polyester, characterized in that: The method comprises the following steps: 1) Preparation of rare earth functional powders: Putting nitrogen-containing compounds, guanidine hydrochloride, rare earth chloride and deionized water into a reaction kettle and stirring them evenly; then adding concentrated sulfuric acid into the reaction kettle to react and obtain an intermediate product; putting the intermediate product into an oven to dry, grinding the dried intermediate product, and then putting it into a muffle furnace to calcine it; 2) Preparation of alcohol-based rare earth functional dispersion: The rare earth functional powder obtained in step 1) and the aliphatic diol are mixed evenly, and added to a sand mill for thorough grinding; then a dispersant is added, and multi-stage grinding is performed in a sand mill to obtain a uniformly dispersed alcohol-based rare earth functional dispersion; 3) Preparation of antibacterial polyester: Weigh the alcohol-based rare earth functional dispersion, aliphatic diol, dibasic acid, stabilizer and catalyst according to mass to prepare a polymerization slurry, put it into a high-pressure reactor for esterification and polycondensation reaction to obtain a rare earth functional polyester melt; cool and pelletize the obtained rare earth functional polyester melt, and transport it to a solid phase viscosity increasing system for crystallization and solid phase polycondensation reaction to obtain antibacterial polyester chips; The rare earth functional powder comprises 5-30 parts by weight of a nitrogen-containing compound, 15-80 parts by weight of guanidine hydrochloride, 35-65 parts by weight of a rare earth chloride, and 50-200 parts by weight of deionized water; 3-25 mL of concentrated sulfuric acid is added; The nitrogen-containing compound is a mixture of melamine, dicyandiamide and urea, wherein the molar ratio of melamine, dicyandiamide and urea is 1-3:6-8:1; The rare earth chloride is a mixture of lanthanum chloride and one of cerium chloride, yttrium chloride or gadolinium chloride, and the molar ratio of lanthanum chloride to cerium chloride / yttrium chloride / gadolinium chloride is 3-5:1-2.
2. The method for preparing the antibacterial polyester according to claim 1, characterized in that: In step 1), the temperature of the reactor is 70-150°C, and the stirring is performed for 3-8 hours; the drying temperature is 100-200°C; the calcination temperature is 300-1000°C, and the time is 2-7 hours.
3. The method for preparing the antibacterial polyester according to claim 1, characterized in that: The alcohol-based rare earth functional dispersion comprises 20-35 parts of rare earth functional powder, 60-79 parts of aliphatic diol and 1-5 parts of dispersant by weight; the particle size of the alcohol-based rare earth functional dispersion is 100-300nm; the dispersant is one or a mixture of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate, modified styrene maleic acid copolymer solution, modified polymer block copolymer and high molecular weight silane copolymer containing pigment affinity group.
4. The method for preparing the antibacterial polyester according to claim 1, characterized in that: In step 3), the esterification reaction temperature is 220-300°C, the polycondensation reaction temperature is 240-300°C, the crystallization temperature is 130-190°C, and the solid phase polycondensation reaction temperature is 180-220°C.
5. The method for preparing the antibacterial polyester according to claim 1, characterized in that: The aliphatic diol in step 2) and step 3) is the same substance, and the aliphatic diol is any one of ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol and decanediol.
6. The method for preparing the antibacterial polyester according to claim 1, characterized in that: In step 3), the dibasic acid is one or a mixture of two of terephthalic acid, isophthalic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid and sebacic acid; The stabilizer is a mixture of one or more of trimethyl phosphite, trimethyl phosphate, triphenyl phosphate, triethyl phosphate, and bis(2,4-dicumylphenyl)pentaerythritol-diphosphite; The catalyst is a mixture of one or more antimony catalysts, titanium catalysts, and germanium catalysts. The antimony catalyst is one or more of ethylene glycol antimony, antimony trioxide, or antimony acetate. The titanium catalyst is one or more of tetrabutyl titanate, ethylene glycol titanium, tetraisopropyl titanate, Ti / Zn catalyst, and titanic acid. The germanium catalyst is germanium dioxide.
7. The method for preparing the antibacterial polyester according to claim 1, characterized in that: In step 3), the molar ratio of the dibasic acid to the aliphatic diol is 1:1.1-1.7, the mass of the stabilizer is 0.003-0.05% of the total mass of the polymerization slurry, the mass of the catalyst is 0.02-0.15% of the total mass of the polymerization slurry, and the rare earth functional powder accounts for 0.5%-5% of the total mass of the polymerization slurry.
8. An antibacterial polyester prepared by the preparation method according to any one of claims 1 to 7.
9. The use of the antibacterial polyester as claimed in claim 8 in antibacterial functional fibers, medical mattresses, and packaging films, characterized in that: The intrinsic viscosity of the polyester chips is 0.6-1.4 dL / g. The antibacterial polyester chips are made into corresponding fibers, plastics and films for application.