A nylon large biological fiber containing antioxidant active ingredients and preparation method thereof
By combining the antioxidant active ingredients in buckwheat leaves and yucca extract with Zn/Ce bimetallic components, the binding stability of the antioxidant active ingredients of nylon fiber is improved, and the acid dyeing of antioxidant active ingredients in the prior art is solved. The problem of reduced stability during the process achieves better dyeing effect and water washing resistance.
Patent Information
- Application Number
- CN202411178586.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-27
AI Technical Summary
In the prior art, in the antioxidant functional modification of plant extracts to nylon fibers, the binding performance of the antioxidant active ingredient and nylon fibers is poor, resulting in a decrease in the stability of the active ingredient and easy deactivation during the acid dyeing process. Dyeing effect and water-resistant performance.
The antioxidant active ingredients in buckwheat leaves and yucca extract were combined with the Zn/Ce bimetallic composition, and the binding stability and compatibility of the antioxidant active ingredients were improved through porous base carrier and amino acid treatment, and combined with spinning. Technology prepares nylon large biofibers containing antioxidant active ingredients.
The binding performance and stability of the antioxidant active ingredients and nylon fibers are improved, the failure of the active ingredients during the acid dyeing process is avoided, the dyeing uniformity and water washing resistance are enhanced, and the antibacterial and physical properties of the fibers are improved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of nylon fibers, in particular to a nylon large biological fiber containing antioxidant active ingredients and a preparation method thereof. Background Art
[0002] Nylon fiber, also known as Polyamide in English and polyamide in scientific name, is the first synthetic fiber in the world. Its invention can be traced back to the 1930s, when it was created by American chemist Carothers and his research team. Nylon fiber has extremely high wear resistance, ranking first among all kinds of fabrics. It is about 10 times more wear-resistant than cotton and about 20 times more wear-resistant than wool. Adding a small amount of nylon fiber to blended fabrics can greatly improve the wear resistance of the fabric. At the same time, nylon fiber also has good strength, elasticity and hygroscopicity. When nylon fiber is stretched to 103-106%, the elastic recovery rate can reach 100%. The fabric made of it can withstand a certain amount of pressure and tension, and the wearing feeling and touch of the ready-made clothes are better than those of polyester fabrics. In the prior art, nylon fiber is used in the fields of clothing, industrial production, medical treatment, etc. In the field of clothing, nylon fiber is widely used in the production of sportswear, outdoor clothing, underwear, socks, etc. due to its wear resistance, strength and good elasticity. In addition, nylon fiber can also be blended with other fibers to produce clothing of various styles. In the field of industrial production, the high strength and high wear resistance of nylon fiber make it an ideal choice for industrial fabrics, and it is widely used in the production of cord fabrics, cables, conveyor belts, fishing nets, etc.
[0003] With the development of science and technology and the improvement of living standards, the basic properties of nylon fibers have gradually been unable to meet the diverse application requirements. There are more and more studies on the functional improvement of nylon, and functional nylon fibers are constantly being innovated, which is of great significance to the functional research and application expansion of nylon fibers.
[0004] Since tea contains tea polyphenols, catechins and other antioxidant active ingredients, orange peel contains hesperidin, naringin and other antioxidant active ingredients, and knotweed and grapes contain polyphenol compounds, flavonoid compounds, resveratrol and other antioxidant active ingredients, which have ideal antioxidant properties, the prior art has disclosed the use of the above plant extracts containing antioxidant active ingredients to modify the antioxidant function of nylon fiber. However, in the use of plant extracts to modify the antioxidant function of nylon fiber, the antioxidant active ingredients in the plant extracts have poor binding performance with the nylon fiber; in the subsequent dyeing process for nylon fiber, in order to achieve the ideal dyeing effect, it is necessary to cooperate with the dye in an acidic environment with a pH value of 4-5; this not only leads to reduced stability of the active ingredients in the plant extracts, which are easy to fail and fail to achieve the desired antioxidant properties, but also leads to reduced dyeing effect and easy to cause uneven dyeing. At the same time, during the multiple washing processes of nylon fibers, the antioxidant active ingredients are easily lost and the water washing resistance is poor; and when the antioxidant functionality of nylon fibers is modified using plant extracts, the addition of plant extracts will also affect the physical properties of nylon fibers. Summary of the invention
[0005] In order to solve the technical problems existing in the prior art, the present invention provides a nylon large biofiber containing antioxidant active ingredients and a preparation method thereof, which can improve the binding performance of the active ingredients of plant extracts with antioxidant function and nylon fibers, effectively avoid the problem of reduced stability and easy inactivation of the active ingredients of plant extracts during acid dyeing; and effectively avoid the problem of the active ingredients of plant extracts affecting the dyeing effect and causing uneven dyeing; and further improve the water washing resistance and physical properties of nylon fibers.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing nylon large biofiber containing antioxidant active ingredients comprises the following steps: preparing buckwheat leaf extract, preparing yucca extract, preparing a porous base carrier, amination treatment, modification treatment, loading, preparing functional masterbatch, and spinning.
[0008] The method for preparing the buckwheat leaf extract comprises the following steps: placing clean buckwheat leaves in a -40°C to -35°C environment for 42-48 hours of static freezing, freeze-drying them in a low-temperature freeze dryer for 22-24 hours, and then grinding them at 9000-10000 rpm to obtain buckwheat leaf powder with a particle size of 1700-1800 meshes; then putting the buckwheat leaf powder into an ethanol solution (volume concentration of 55-60%) with a weight of 10-12 times, performing a first ultrasonic extraction for 15-20 minutes, and filtering to obtain a first extract; putting the filter residue into an ethanol solution (volume concentration of 55-60%) with a weight of 8-10 times, performing a second ultrasonic extraction for 10-15 minutes, and filtering to obtain a second extract; combining the first extract and the second extract, and concentrating them at 62-65°C to 42-45% of the original volume in a vacuum environment of 0.06-0.07 MPa to obtain the buckwheat leaf extract.
[0009] In the preparation of the buckwheat leaf extract, the ultrasonic extraction temperature is controlled to be 40-45° C., the ultrasonic extraction frequency is controlled to be 41-43 kHz, and the ultrasonic extraction power is controlled to be 200-250W.
[0010] Buckwheat (Fagopyrum esculentum Moench), also known as black wheat and triangle wheat, is a dicotyledonous annual herb belonging to the genus Fagopyrum. It likes cold weather and is resistant to barrenness. Buckwheat leaves are rich in flavonoids (such as rutin, quercetin, etc.), which are natural antioxidant active ingredients with good antioxidant properties; and the content of flavonoids in buckwheat leaves is higher than that in buckwheat seeds. At the same time, buckwheat leaves also have the effects of clearing heat and detoxification, antibacterial and anti-inflammatory.
[0011] The method for preparing the yucca extract comprises the following steps: placing clean yucca stems and leaves in a -40°C to -35°C environment for freezing for 42-48 hours, freeze-drying them in a low-temperature freeze dryer for 22-24 hours, and then crushing them at 9000-10000 rpm to obtain yucca powder with a particle size of 1700-1800 meshes; then putting the yucca powder into an ethanol solution (volume concentration of 55-60%) with a weight of 13-15 times, performing a first ultrasonic extraction for 15-20 minutes, and filtering to obtain a first extract; putting the filter residue into an ethanol solution (volume concentration of 55-60%) with a weight of 10-12 times, performing a second ultrasonic extraction for 10-15 minutes, and filtering to obtain a second extract; combining the first extract and the second extract, and concentrating them at 62-65°C to 58-60% of the original volume in a vacuum environment of 0.06-0.07 MPa to obtain the yucca extract.
[0012] In the preparation of the yucca extract, the ultrasonic extraction temperature is controlled to be 40-45° C., the ultrasonic extraction frequency is controlled to be 41-43 kHz, and the ultrasonic extraction power is controlled to be 200-250W.
[0013] Yucca smalliana Fern, also known as soft-leaf yucca, hairy-edge yucca, and pineapple, is a plant of the genus Yucca in the Asparagaceae family. The antioxidant active ingredients in the stems and leaves of yucca mainly include flavonoids, polyphenols, saponins, etc. The aforementioned antioxidant active ingredients can show good antioxidant properties through different mechanisms; at the same time, yucca also has antibacterial, detoxifying, and anti-inflammatory effects.
[0014] The method for preparing the porous base carrier comprises the following steps: adding 2-methylimidazole into 18-20 times the weight of anhydrous methanol, stirring and dissolving to obtain a first liquid for standby use; adding zinc nitrate hexahydrate and cerium nitrate hexahydrate into 22-24 times the weight of anhydrous methanol, stirring and dissolving to obtain a second liquid for standby use; adding the second liquid into the first liquid under stirring conditions, stirring at room temperature for 50-60 minutes, and standing for 20-30 minutes to obtain a reaction liquid; centrifuging and separating at 11000-12000 rpm to obtain a solid, washing the solid with 2-2.5 times the weight of anhydrous methanol, placing the solid in a vacuum drying oven, drying at 65-70° C. to constant weight in a vacuum environment of 0.085-0.095 MPa, and grinding the solid to obtain a porous base carrier.
[0015] In the preparation of the porous base carrier, the molar ratio of 2-methylimidazole, zinc nitrate hexahydrate and cerium nitrate hexahydrate is 2.2-2.3:0.7-0.8:0.35-0.4.
[0016] The amination treatment method comprises the following steps: putting the porous base carrier into an ethanol solution (volume concentration of 75-80%) of 6-7 times its weight, ultrasonically dispersing the porous base carrier for 5-10 minutes, stirring and heating the solution to 40-45° C., keeping the solution warm and stirring for 10-15 minutes, stirring and dripping the bisaminosilane coupling agent A-2120, and controlling the dripping time of the bisaminosilane coupling agent A-2120 to be 40-50 minutes; after the dripping is completed, keeping the solution warm and stirring for 5-6 hours, centrifuging at 11000-12000 rpm to obtain a solid, washing the solid with 2.5-3 times its weight of deionized water, placing the solid in a vacuum drying oven, drying the solution at 90-95° C. to a constant weight in a vacuum environment of 0.085-0.095 MPa, and grinding the solution evenly to obtain an amination carrier.
[0017] In the amination treatment, the weight ratio of the porous base carrier to the bisaminosilane coupling agent A-2120 is 1:0.16-0.19.
[0018] The modification treatment method comprises the following steps: adding adipoyl chloride into a reactor filled with tetrahydrofuran, stirring and dissolving, replacing the air in the reactor with nitrogen, adding an amination carrier with stirring, stirring at room temperature for 10-12 hours, centrifuging at 11000-12000 rpm to obtain a solid, washing the solid with 1.5-1.8 times the weight of tetrahydrofuran, filtering out the solid, adding the solid into a reactor filled with N,N-dimethylformamide, replacing the air in the reactor with nitrogen, adding 1,2-ethanedithiol and triethylamine with stirring, stirring at room temperature for 5-6 hours, centrifuging at 11000-12000 rpm to obtain a solid, washing the solid with 3-3.5 times the weight of deionized water for 2-3 times, placing the solid in a vacuum drying oven, drying at 110-120° C. to constant weight in a vacuum environment of 0.085-0.095 MPa, grinding the solid uniformly, and obtaining a modified carrier.
[0019] In the modification treatment, the weight ratio of adipoyl chloride, amination carrier, 1,2-ethanedithiol, and triethylamine is 4-4.2:25-26:0.5-0.55:0.9-0.95;
[0020] The weight ratio of the amination carrier to tetrahydrofuran is 1:8-9;
[0021] The weight ratio of the amination carrier to N,N-dimethylformamide is 1:4-5.
[0022] The loading method comprises the following steps: uniformly mixing equal volumes of a buckwheat leaf extract and a yucca extract to obtain a loading liquid; then adding the modified carrier into the loading liquid, performing ultrasonic dispersion for 10-20 minutes, stirring and heating to 35-40° C., maintaining the temperature and stirring for 5-6 hours, and centrifuging at 11000-12000 rpm to obtain a solid; washing the solid with 3-3.5 times the weight of deionized water, placing the solid in a vacuum drying oven, drying at 80-85° C. to a constant weight in a vacuum environment of 0.04-0.05 MPa, and grinding the solid to obtain a composite active ingredient.
[0023] In the loading, the weight ratio of the modified carrier to the loading liquid is 1:6-6.5;
[0024] The method for preparing the functional masterbatch is to put the composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate into a twin-screw extruder, heat it to 260-265° C., keep it warm and melt for 25-35 minutes, and then extrude and granulate it to obtain the functional masterbatch.
[0025] In the functional masterbatch, the weight ratio of the composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate is 11-12:83-86:0.9-1.1:0.7-0.8:0.65-0.75.
[0026] The spinning method is to put nylon 66 chips and functional masterbatch into a spinning melting device, extrude and melt them in a temperature environment of 260-265°C, use a screw spinning machine to spin them, and control the spinning speed to be 1700-1850m / min, and then stretch, oil and wind them to obtain nylon large bio-fibers containing antioxidant active ingredients.
[0027] In the spinning, the weight ratio of nylon 66 chips to functional masterbatch is 100:11-12.
[0028] A nylon large biological fiber containing antioxidant active ingredients is prepared by adopting the above-mentioned preparation method.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The method for preparing nylon large biofiber containing antioxidant active ingredients of the present invention is aimed at the characteristics of nylon fiber and the characteristics of antioxidant active ingredients in buckwheat leaves and yucca. In the step of preparing a porous base carrier, a Zn / Ce bimetallic component is used to combine with an organic ligand 2-methylimidazole. Through the synergistic coordination effect of the Zn / Ce bimetallic active center, the active sites in the prepared porous base carrier are improved, and the subsequent binding stability with the antioxidant active ingredients is improved; then in the amination treatment step, a bisaminosilane coupling agent is used to aminate the porous base carrier to effectively introduce amino groups, which, on the one hand, improves the subsequent modification treatment effect, ensures the binding effect of the modified carrier with the antioxidant active ingredients, and improves the stability of the antioxidant active ingredients in the nylon fiber; on the other hand, it improves the compatibility and binding performance of the composite active ingredients containing the antioxidant active ingredients with nylon; then in the modification treatment step, the aminated carrier is subjected to thiol modification The modified carrier is subjected to a treatment to further improve the stability and durability of the combination between the modified carrier and the antioxidant active ingredient, thereby improving its functional stability in the nylon fiber; then in the loading step, buckwheat leaf extract and yucca extract containing antioxidant active ingredients such as flavonoids and polyphenols are selected, and the buckwheat leaf extract and the yucca extract are mixed to form a loading liquid, and then the modified carrier is used for adsorption and bonding loading process to obtain a composite active ingredient; then the composite active ingredient is used to make a functional masterbatch, which is then spun with nylon raw materials to obtain a nylon bio-fiber containing antioxidant active ingredients; the combination performance of the active ingredients of plant extracts with antioxidant function and nylon fibers can be improved, and the problem of reduced stability and easy inactivation of antioxidant active ingredients during acid dyeing can be effectively avoided; and the antioxidant active ingredients can be effectively avoided from affecting the dyeing effect and the problem of uneven dyeing can be avoided; and the water washing resistance and physical properties of the nylon bio-fiber can be further improved.
[0031] (2) The nylon biofiber containing antioxidant active ingredients of the present invention has a DPPH free radical scavenging rate of 90.0-90.4%, and ABTS + The free radical scavenging rate is 88.4-88.7%, the hydroxyl radical scavenging rate is 80.9-81.2%, the breaking strength is 5.8-6.1cN / dtex, and the breaking elongation is 24.8-25.1%.
[0032] (3) The nylon biofiber containing antioxidant active ingredients of the present invention has an antibacterial rate of 99.3-99.5% against Staphylococcus aureus, an antibacterial rate of 98.7-99.0% against Escherichia coli, and an antibacterial rate of 95.3-95.6% against Candida albicans.
[0033] (4) The nylon biofiber containing antioxidant active ingredients of the present invention has a dyeing percentage of 97.1-97.3%, a half-dyeing time extension rate of 3.8-4.0%, a dyeing color difference value △E of 0.03-0.04, and a color fastness to soaping of grade 4.
[0034] (5) The nylon biofiber containing antioxidant active ingredients of the present invention has a DPPH free radical scavenging rate of 89.2-89.7% after dyeing, and ABTS + The free radical scavenging rate was 87.6-88.1%, the hydroxyl radical scavenging rate was 80.0-80.4%, the antibacterial rate of Staphylococcus aureus was 98.1-98.5%, the antibacterial rate of Escherichia coli was 97.7-98.1%, and the antibacterial rate of Candida albicans was 94.1-94.5%.
[0035] (6) The nylon biofiber containing antioxidant active ingredients of the present invention has a DPPH free radical scavenging rate of 83.0-83.6% after repeated washing 20 times, and ABTS + The free radical scavenging rate was 81.4-81.9%, the hydroxyl radical scavenging rate was 74.8-75.2%, the antibacterial rate of Staphylococcus aureus was 90.7-91.4%, the antibacterial rate of Escherichia coli was 90.6-91.0%, and the antibacterial rate of Candida albicans was 87.4-87.7%. DETAILED DESCRIPTION
[0036] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0037] Example 1
[0038] This embodiment provides a method for preparing a nylon large biofiber containing antioxidant active ingredients, specifically:
[0039] 1. Preparation of Buckwheat Leaf Extract
[0040] The clean buckwheat leaves were frozen at -40°C for 42 hours, freeze-dried in a low-temperature freeze dryer for 22 hours, and then crushed at 9000rpm to buckwheat leaf powder with a particle size of 1700 mesh; the buckwheat leaf powder was then put into 10 times the weight of an ethanol solution (volume concentration of 55%), subjected to a first ultrasonic extraction for 15 minutes, and filtered to obtain a first extract; the filter residue was put into 8 times the weight of an ethanol solution (volume concentration of 55%), subjected to a second ultrasonic extraction for 10 minutes, and filtered to obtain a second extract; the first extract and the second extract were combined, and concentrated to 42% of the original volume at 62°C in a vacuum environment of 0.06MPa to obtain a buckwheat leaf extract.
[0041] The ultrasonic extraction temperature was controlled to be 40°C, the ultrasonic extraction frequency was 41kHz, and the ultrasonic extraction power was 200W.
[0042] 2. Preparation of Yucca Extract
[0043] The clean yucca stems and leaves were frozen at -40°C for 42 hours, freeze-dried in a low-temperature freeze dryer for 22 hours, and then crushed at 9000rpm to obtain yucca powder with a particle size of 1700 mesh; the yucca powder was then put into 13 times the weight of an ethanol solution (volume concentration of 55%), subjected to a first ultrasonic extraction for 15 minutes, and filtered to obtain a first extract; the filter residue was put into 10 times the weight of an ethanol solution (volume concentration of 55%), subjected to a second ultrasonic extraction for 10 minutes, and filtered to obtain a second extract; the first extract and the second extract were combined, and concentrated to 58% of the original volume at 62°C in a vacuum environment of 0.06MPa to obtain a yucca extract.
[0044] The ultrasonic extraction temperature was controlled to be 40°C, the ultrasonic extraction frequency was 41kHz, and the ultrasonic extraction power was 200W.
[0045] 3. Preparation of porous base carrier
[0046] The first liquid is prepared by adding 2-methylimidazole into 18 times the weight of anhydrous methanol, stirring and dissolving, and the first liquid is prepared for standby use; zinc nitrate hexahydrate and cerium nitrate hexahydrate are added into 22 times the weight of anhydrous methanol, stirring and dissolving, and the second liquid is prepared for standby use; the second liquid is added into the first liquid under stirring conditions, and after stirring at room temperature for 50 minutes, the reaction liquid is allowed to stand for 20 minutes to obtain a reaction liquid; a solid is obtained by centrifugation at 11000 rpm, and the solid is washed with 2 times the weight of anhydrous methanol, placed in a vacuum drying oven, dried at 65°C to constant weight in a vacuum environment of 0.085 MPa, and ground evenly to obtain a porous base carrier.
[0047] Wherein, the molar ratio of 2-methylimidazole, zinc nitrate hexahydrate and cerium nitrate hexahydrate is 2.2:0.7:0.35.
[0048] 4. Amination treatment
[0049] The porous base carrier was put into 6 times the weight of ethanol solution (volume concentration of 75%), and after ultrasonic dispersion for 5 minutes, the temperature was raised to 40°C with stirring, and after keeping warm and stirring for 10 minutes, the bisaminosilane coupling agent A-2120 was added dropwise with stirring, and the addition time of the bisaminosilane coupling agent A-2120 was controlled to be 40 minutes; after the addition was completed, the solution was kept warm and stirred for 5 hours, and then centrifuged at 11000 rpm to obtain a solid. After the solid was washed with 2.5 times the weight of deionized water, it was placed in a vacuum drying oven, dried at 90°C to constant weight in a vacuum environment of 0.085 MPa, and ground evenly to obtain an amino carrier.
[0050] Wherein, the weight ratio of the porous base carrier to the bisaminosilane coupling agent A-2120 is 1:0.16.
[0051] 5. Modification treatment
[0052] Adipoyl chloride was added to a reactor filled with tetrahydrofuran, and after stirring and dissolving, the air in the reactor was replaced with nitrogen, and the amino carrier was added with stirring. After stirring at room temperature for 10 hours, the solid was obtained by centrifugation at 11000 rpm. The solid was washed with 1.5 times the weight of tetrahydrofuran, filtered out and added to a reactor filled with N,N-dimethylformamide, and the air in the reactor was replaced with nitrogen. 1,2-ethanedithiol and triethylamine were added with stirring. After stirring at room temperature for 5 hours, the solid was obtained by centrifugation at 11000 rpm. The solid was washed 3 times with 3 times the weight of deionized water, and then placed in a vacuum drying oven. In a vacuum environment of 0.085 MPa, it was dried at 110°C to constant weight and ground evenly to obtain a modified carrier.
[0053] Wherein, the weight ratio of adipoyl chloride, amination carrier, 1,2-ethanedithiol and triethylamine is 4:25:0.5:0.9.
[0054] The weight ratio of the amination carrier to tetrahydrofuran is 1:8.
[0055] The weight ratio of the amination carrier to N,N-dimethylformamide is 1:4.
[0056] 6. Load
[0057] The buckwheat leaf extract and the yucca extract were mixed in equal volumes to prepare a loading liquid; the modified carrier was then added to the loading liquid, ultrasonically dispersed for 10 minutes, heated to 35°C with stirring, kept warm and stirred for 5 hours, and then centrifuged at 11000 rpm to obtain a solid; the solid was washed with 3 times its weight of deionized water, placed in a vacuum drying oven, dried at 80°C to constant weight in a vacuum environment of 0.04 MPa, and ground evenly to obtain a composite active ingredient.
[0058] Wherein, the weight ratio of the modified carrier to the loading liquid is 1:6.
[0059] 7. Preparation of functional masterbatch
[0060] The composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate were put into a twin-screw extruder, heated to 260°C, kept warm and melted for 25 minutes, and then extruded and granulated to obtain a functional masterbatch.
[0061] Among them, the weight ratio of the composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate is 11:83:0.9:0.7:0.65.
[0062] 8. Spinning
[0063] Nylon 66 chips and functional masterbatch are put into a spinning melting device. After being extruded and melted in a temperature environment of 260°C, they are spun using a screw spinning machine at a controlled spinning speed of 1700m / min. Then, they are stretched, oiled and wound to obtain nylon large bio-fibers containing antioxidant active ingredients.
[0064] Among them, the weight ratio of nylon 66 chips and functional masterbatch is 100:11.
[0065] This embodiment also provides a nylon large biological fiber containing antioxidant active ingredients, which is prepared using the above-mentioned preparation method.
[0066] Example 2
[0067] This embodiment provides a method for preparing a nylon large biofiber containing antioxidant active ingredients, specifically:
[0068] 1. Preparation of Buckwheat Leaf Extract
[0069] The clean buckwheat leaves were frozen at -38°C for 45 hours, freeze-dried in a low-temperature freeze dryer for 23 hours, and then crushed at 9500rpm to buckwheat leaf powder with a particle size of 1750 mesh; the buckwheat leaf powder was then put into 11 times the weight of an ethanol solution (volume concentration of 57%), subjected to a first ultrasonic extraction for 18 minutes, and filtered to obtain a first extract; the filter residue was put into 9 times the weight of an ethanol solution (volume concentration of 57%), subjected to a second ultrasonic extraction for 12 minutes, and filtered to obtain a second extract; the first extract and the second extract were combined, and concentrated to 43% of the original volume at 63°C in a vacuum environment of 0.065MPa to obtain a buckwheat leaf extract.
[0070] The temperature of ultrasonic extraction was controlled to be 42°C, the frequency of ultrasonic extraction was 42kHz, and the power of ultrasonic extraction was 240W.
[0071] 2. Preparation of Yucca Extract
[0072] The clean yucca stems and leaves were frozen at -38°C for 45 hours, freeze-dried in a low-temperature freeze dryer for 23 hours, and then crushed at 9500rpm to obtain yucca powder with a particle size of 1750 mesh; the yucca powder was then put into 14 times the weight of an ethanol solution (volume concentration of 57%), subjected to a first ultrasonic extraction for 18 minutes, and filtered to obtain a first extract; the filter residue was put into 11 times the weight of an ethanol solution (volume concentration of 57%), subjected to a second ultrasonic extraction for 12 minutes, and filtered to obtain a second extract; the first extract and the second extract were combined, and concentrated to 59% of the original volume at 63°C in a vacuum environment of 0.065MPa to obtain a yucca extract.
[0073] The temperature of ultrasonic extraction was controlled to be 42°C, the frequency of ultrasonic extraction was 42kHz, and the power of ultrasonic extraction was 240W.
[0074] 3. Preparation of porous base carrier
[0075] The method comprises the following steps: adding 2-methylimidazole to 19 times the weight of anhydrous methanol, stirring and dissolving, and obtaining a first liquid for standby use; adding zinc nitrate hexahydrate and cerium nitrate hexahydrate to 23 times the weight of anhydrous methanol, stirring and dissolving, and obtaining a second liquid for standby use; adding the second liquid to the first liquid under stirring conditions, stirring at room temperature for 55 minutes, and standing for 25 minutes to obtain a reaction liquid; centrifuging at 11500 rpm to obtain a solid, washing the solid with 2.3 times the weight of anhydrous methanol, placing the solid in a vacuum drying oven, drying at 68°C to constant weight in a vacuum environment of 0.09 MPa, and grinding the solid to obtain a porous base carrier.
[0076] Wherein, the molar ratio of 2-methylimidazole, zinc nitrate hexahydrate and cerium nitrate hexahydrate is 2.25:0.75:0.38.
[0077] 4. Amination treatment
[0078] The porous base carrier was put into 6.5 times the weight of ethanol solution (volume concentration of 78%), and after ultrasonic dispersion for 8 minutes, the temperature was raised to 42°C with stirring, and after keeping warm and stirring for 12 minutes, the bisaminosilane coupling agent A-2120 was added dropwise with stirring, and the addition time of the bisaminosilane coupling agent A-2120 was controlled to be 45 minutes; after the addition was completed, the solution was kept warm and stirred for 5.5 hours, and then centrifuged at 11500rpm to obtain a solid. After the solid was washed with 2.8 times the weight of deionized water, it was placed in a vacuum drying oven, dried at 92°C to constant weight in a vacuum environment of 0.09MPa, and ground evenly to obtain an amino carrier.
[0079] Wherein, the weight ratio of the porous base carrier to the bisaminosilane coupling agent A-2120 is 1:0.18.
[0080] 5. Modification treatment
[0081] Adipoyl chloride was added to a reactor filled with tetrahydrofuran, and after stirring and dissolving, the air in the reactor was replaced with nitrogen, and the amino carrier was added with stirring. After stirring at room temperature for 11 hours, the solid was centrifuged at 11500 rpm to obtain a solid. The solid was washed with 1.6 times the weight of tetrahydrofuran, filtered out and added to a reactor filled with N,N-dimethylformamide, and the air in the reactor was replaced with nitrogen. 1,2-ethanedithiol and triethylamine were added with stirring. After stirring at room temperature for 5.5 hours, the solid was centrifuged at 11500 rpm to obtain a solid. The solid was washed 3 times with 3.2 times the weight of deionized water, and then placed in a vacuum drying oven. In a vacuum environment of 0.09 MPa, it was dried at 115°C to constant weight and ground evenly to obtain a modified carrier.
[0082] Wherein, the weight ratio of adipoyl chloride, amination carrier, 1,2-ethanedithiol and triethylamine is 4.1:25.5:0.53:0.92.
[0083] The weight ratio of the amination carrier to tetrahydrofuran is 1:8.5.
[0084] The weight ratio of the amination carrier to N,N-dimethylformamide is 1:4.5.
[0085] 6. Load
[0086] The buckwheat leaf extract and the yucca extract were mixed in equal volumes to prepare a loading liquid; the modified carrier was then added to the loading liquid, ultrasonically dispersed for 15 minutes, heated to 38°C with stirring, kept warm and stirred for 5.5 hours, and then centrifuged at 11500 rpm to obtain a solid; the solid was washed with 3.2 times its weight of deionized water, placed in a vacuum drying oven, dried at 83°C to constant weight in a vacuum environment of 0.045 MPa, and ground evenly to obtain a composite active ingredient.
[0087] Among them, the weight ratio of the modified carrier to the loading liquid is 1:6.3.
[0088] 7. Preparation of functional masterbatch
[0089] The composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate were put into a twin-screw extruder, heated to 263°C, kept warm and melted for 30 minutes, and then extruded and granulated to obtain a functional masterbatch.
[0090] Among them, the weight ratio of the composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate is 11.5:85:1:0.75:0.7.
[0091] 8. Spinning
[0092] Nylon 66 chips and functional masterbatch are put into a spinning melting device. After being extruded and melted in a temperature environment of 263°C, they are spun using a screw spinning machine at a controlled spinning speed of 1800m / min. Then, they are stretched, oiled and wound to obtain nylon large bio-fibers containing antioxidant active ingredients.
[0093] Among them, the weight ratio of nylon 66 chips and functional masterbatch is 100:11.7.
[0094] This embodiment also provides a nylon large biological fiber containing antioxidant active ingredients, which is prepared using the above-mentioned preparation method.
[0095] Example 3
[0096] This embodiment provides a method for preparing a nylon large biofiber containing antioxidant active ingredients, specifically:
[0097] 1. Preparation of Buckwheat Leaf Extract
[0098] The clean buckwheat leaves were frozen at -35°C for 48 hours, freeze-dried in a low-temperature freeze dryer for 24 hours, and then crushed at 10000 rpm to obtain buckwheat leaf powder with a particle size of 1800 mesh; the buckwheat leaf powder was then put into an ethanol solution (volume concentration of 60%) with a weight of 12 times, and the first ultrasonic extraction was performed for 20 minutes, and the first extract was obtained by filtering; the filter residue was put into an ethanol solution (volume concentration of 60%) with a weight of 10 times, and the second ultrasonic extraction was performed for 15 minutes, and the second extract was obtained by filtering; the first extract and the second extract were combined, and concentrated to 45% of the original volume at 65°C in a vacuum environment of 0.07 MPa to obtain a buckwheat leaf extract.
[0099] The ultrasonic extraction temperature was controlled at 45°C, the ultrasonic extraction frequency was 43kHz, and the ultrasonic extraction power was 250W.
[0100] 2. Preparation of Yucca Extract
[0101] The clean yucca stems and leaves were frozen at -35°C for 48 hours, freeze-dried in a low-temperature freeze dryer for 24 hours, and then crushed at 10,000 rpm to obtain yucca powder with a particle size of 1800 mesh; the yucca powder was then put into an ethanol solution (volume concentration of 60%) with a weight of 15 times, and the first ultrasonic extraction was performed for 20 minutes, and the first extract was obtained by filtering; the filter residue was put into an ethanol solution (volume concentration of 60%) with a weight of 12 times, and the second ultrasonic extraction was performed for 15 minutes, and the second extract was obtained by filtering; the first extract and the second extract were combined, and concentrated to 60% of the original volume at 65°C in a vacuum environment of 0.07 MPa to obtain a yucca extract.
[0102] The ultrasonic extraction temperature was controlled at 45°C, the ultrasonic extraction frequency was 43kHz, and the ultrasonic extraction power was 250W.
[0103] 3. Preparation of porous base carrier
[0104] Put 2-methylimidazole into 20 times the weight of anhydrous methanol, stir and dissolve to obtain a first liquid for standby use; put zinc nitrate hexahydrate and cerium nitrate hexahydrate into 24 times the weight of anhydrous methanol, stir and dissolve to obtain a second liquid for standby use; put the second liquid into the first liquid under stirring conditions, stir at room temperature for 60 minutes, and then stand for 30 minutes to obtain a reaction liquid; centrifuge at 12000rpm to obtain a solid, wash the solid with 2.5 times the weight of anhydrous methanol, place it in a vacuum drying oven, dry it at 70°C to constant weight in a vacuum environment of 0.095MPa, and grind it evenly to obtain a porous base carrier.
[0105] Wherein, the molar ratio of 2-methylimidazole, zinc nitrate hexahydrate and cerium nitrate hexahydrate is 2.3:0.8:0.4.
[0106] 4. Amination treatment
[0107] The porous base carrier was put into 7 times the weight of ethanol solution (volume concentration of 80%), and after ultrasonic dispersion for 10 minutes, the temperature was raised to 45°C with stirring, and after keeping warm and stirring for 15 minutes, the bisaminosilane coupling agent A-2120 was added dropwise with stirring, and the addition time of the bisaminosilane coupling agent A-2120 was controlled to be 50 minutes; after the addition was completed, the solution was kept warm and stirred for 6 hours, and then centrifuged at 12000 rpm to obtain a solid. After the solid was washed with 3 times the weight of deionized water, it was placed in a vacuum drying oven, dried at 95°C to constant weight in a vacuum environment of 0.095 MPa, and ground evenly to obtain an amino carrier.
[0108] Wherein, the weight ratio of the porous base carrier to the bisaminosilane coupling agent A-2120 is 1:0.19.
[0109] 5. Modification treatment
[0110] Adipoyl chloride was added to a reactor filled with tetrahydrofuran, and after stirring and dissolving, the air in the reactor was replaced by nitrogen, and the amino carrier was added with stirring. After stirring at room temperature for 12 hours, the solid was obtained by centrifugation at 12000 rpm. The solid was washed with 1.8 times the weight of tetrahydrofuran, filtered out and added to a reactor filled with N,N-dimethylformamide, and the air in the reactor was replaced by nitrogen. 1,2-ethanedithiol and triethylamine were added with stirring. After stirring at room temperature for 6 hours, the solid was obtained by centrifugation at 12000 rpm. The solid was washed 3 times with 3.5 times the weight of deionized water, and then placed in a vacuum drying oven. In a vacuum environment of 0.095 MPa, it was dried at 120°C to constant weight and ground evenly to obtain a modified carrier.
[0111] Wherein, the weight ratio of adipoyl chloride, amination carrier, 1,2-ethanedithiol and triethylamine is 4.2:26:0.55:0.95.
[0112] The weight ratio of the amination carrier to tetrahydrofuran is 1:9.
[0113] The weight ratio of the amination carrier to N,N-dimethylformamide is 1:5.
[0114] 6. Load
[0115] The buckwheat leaf extract and the yucca extract were mixed in equal volumes to prepare a loading liquid; the modified carrier was then added to the loading liquid, ultrasonically dispersed for 20 minutes, heated to 40°C with stirring, kept warm and stirred for 6 hours, and then centrifuged at 12000 rpm to obtain a solid; the solid was washed with 3.5 times its weight of deionized water, placed in a vacuum drying oven, dried at 85°C to constant weight in a vacuum environment of 0.05 MPa, and ground evenly to obtain a composite active ingredient.
[0116] Wherein, the weight ratio of the modified carrier to the loading liquid is 1:6.5.
[0117] 7. Preparation of functional masterbatch
[0118] The composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate were put into a twin-screw extruder, heated to 265°C, kept warm and melted for 35 minutes, and then extruded and granulated to obtain a functional masterbatch.
[0119] Among them, the weight ratio of the composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate is 12:86:1.1:0.8:0.75.
[0120] 8. Spinning
[0121] Nylon 66 chips and functional masterbatch are put into a spinning melting device. After being extruded and melted in a temperature environment of 265°C, they are spun using a screw spinning machine at a controlled spinning speed of 1850m / min. Then, they are stretched, oiled and wound to obtain nylon large bio-fibers containing antioxidant active ingredients.
[0122] Among them, the weight ratio of nylon 66 chips and functional masterbatch is 100:12.
[0123] This embodiment also provides a nylon large biological fiber containing antioxidant active ingredients, which is prepared using the above-mentioned preparation method.
[0124] Comparative Example 1
[0125] The technical solution of Example 2 is adopted, but the differences are: 1) the step of preparing buckwheat leaf extract is omitted, and in the subsequent loading step, yucca extract is used as the loading liquid; 2) in the amination treatment, silane coupling agent KH-550 is used instead of bisaminosilane coupling agent A-2120.
[0126] Comparative Example 2
[0127] The technical solution of Example 2 is adopted, except that: 1) the step of preparing the porous base carrier is omitted, and 3A zeolite powder is used to replace the porous base carrier in the subsequent steps. 2) the amination step is omitted, and the dried 3A zeolite powder is directly used in the modification step.
[0128] Comparative Example 3
[0129] The technical solution of Example 2 is adopted, except that: 1) in the step of preparing the porous base carrier, the addition of cerium nitrate hexahydrate is omitted, and the molar ratio of 2-methylimidazole to zinc nitrate hexahydrate is controlled to be 2.25:1.05. 2) the modification treatment step is omitted, and the amination carrier prepared in the amination treatment is directly used in the loading step.
[0130] The antioxidant properties and physical properties of the nylon fibers of Examples 1-3 and Comparative Examples 1-3 were tested respectively, and the DPPH free radical scavenging rate, ABTS + Free radical scavenging rate, hydroxyl radical scavenging rate, breaking strength, and breaking elongation.
[0131] Specifically, the detection method of DPPH free radical scavenging rate is as follows: weigh 2.5 mg of 1,1-diphenyl-2-trinitrophenylhydrazine DPPH, dissolve it in an appropriate amount of anhydrous ethanol, shake it in the dark to make it fully dissolved, and then make up to 100.0 mL with anhydrous ethanol to prepare a DPPH ethanol solution with a concentration of 25.0 mg / L.
[0132] 2.0 g of nylon fibers of Examples 1-3 and Comparative Examples 1-3 were respectively weighed and put into an ultrasonic extraction bottle containing 50 mL of ethanol solution (volume concentration 60%). After soaking for 16 hours, ultrasonic extraction was performed for 10 minutes. The filtrate was then collected by suction filtration using a Buchner funnel. The filtrate was transferred to a rotary evaporator, and the rotary evaporation temperature was controlled to 55° C. and the rotary evaporation vacuum was controlled to 0.085 MPa. When the filtrate was rotary evaporated to 2 mL, the rotary evaporation was stopped, and the ethanol solution (volume concentration 60%) was used to dilute it to 4 mL as the test solution.
[0133] 1 mL of the test solution was added to 2 mL of DPPH ethanol solution, mixed evenly, and allowed to stand in the dark for 10 min. The absorbance at a wavelength of 517 nm was detected using a spectrophotometer to calculate the DPPH free radical scavenging rate.
[0134] ABTS + The free radical scavenging rate was detected as follows: 200.0 mg of 2,2-azino-bis(3-ethyl-benzothiazole-6-sulfonic acid) diammonium salt ABTS and 34.4 mg of potassium persulfate were weighed and dissolved in 50.0 mL of deionized water. The mixture was placed at room temperature in the dark for 24 h to obtain the ABTS mother solution. An appropriate amount of the ABTS mother solution was diluted with an ethanol solution having a volume concentration of 95% to an absorbance of 0.70 at a wavelength of 734 nm to obtain the ABTS diluent.
[0135] The test solution was prepared in the same manner as the test solution preparation method in the aforementioned DPPH·free radical scavenging rate test.
[0136] Add 0.5 mL of the test solution to 5 mL of ABTS diluent, mix well, and place in a dark place for 10 min. Use a spectrophotometer to measure the absorbance at a wavelength of 734 nm and calculate the ABTS + Free radical scavenging rate.
[0137] The hydroxyl radical scavenging rate was detected by the o-phenanthroline method.
[0138] For the specific test methods of breaking strength and breaking elongation, please refer to the national standard GB / T14344-2022 "Test method for tensile properties of chemical fiber filaments".
[0139] The specific results are shown in the following table:
[0140]
[0141] Furthermore, the antibacterial properties of the nylon fibers of Examples 1-3 and Comparative Examples 1-3 were tested respectively, and the specific methods were referred to the relevant provisions in GB / T20944.3-2008 "Evaluation of Antibacterial Properties of Textiles Part 3: Oscillation Method".
[0142] The bacteria used in the antibacterial performance test are: Staphylococcus aureus Staphylococcus aureus (ATCC6538), Escherichia coli Escherichia coli (ATCC 8739), Candida albicans Candida albicans (ATCC10231).
[0143] The specific results are shown in the following table:
[0144]
[0145] Furthermore, the nylon fibers of Examples 1-3 and Comparative Examples 1-3 were dyed, and the dyeing percentage, half-dyeing time extension rate, dyeing color difference value, and soap-resistant color fastness grade were tested. Among them, the calculation of the half-dyeing time extension rate is based on the half-dyeing time of conventional nylon 66 fiber as the reference value, and the half-dyeing time of the nylon fibers of Examples 1-3 and Comparative Examples 1-3 added with antioxidant active ingredients is calculated with the aforementioned reference value to evaluate the effect of the antioxidant active ingredient (i.e., composite active ingredient) on the dyeing performance of the nylon fiber after modification in the present invention.
[0146] The calculation method of the half-dyeing time extension rate is: [(half-dyeing time of nylon fiber modified with antioxidant active ingredients - reference value) / reference value]×100%.
[0147] The specific results are shown in the following table:
[0148]
[0149] Furthermore, the DPPH· free radical scavenging rate, ABTS + The free radical scavenging rate, hydroxyl radical scavenging rate, and antibacterial performance were tested. The specific results are shown in the following table:
[0150]
[0151] Furthermore, the nylon fibers of Examples 1-3 and Comparative Examples 1-3 were respectively spun into fabrics and cut into 20 cm×20 cm washing samples; the washed samples were respectively put into a washing machine, the washing water temperature was set to 45°C, and each washing was performed for 30 minutes, and after the washing was completed, they were placed in a constant temperature environment at 35°C to dry naturally; after repeating the aforementioned washing-drying process 20 times, the DPPH·free radical scavenging rate and ABTS of each nylon fiber after dyeing were respectively measured. + The free radical scavenging rate, hydroxyl radical scavenging rate, and antibacterial performance were tested. The specific results are shown in the following table:
[0152]
[0153] It can be seen that the preparation method of nylon large biofiber containing antioxidant active ingredients of the present invention is aimed at the characteristics of nylon fiber and antioxidant active ingredients. In the step of preparing a porous base carrier, a Zn / Ce bimetallic component is used to combine with an organic ligand 2-methylimidazole, and the synergistic coordination effect of the Zn / Ce bimetallic active center is used to improve the active sites in the prepared porous base carrier, and the subsequent binding stability with the antioxidant active ingredient is improved; then in the amination treatment step, a bisaminosilane coupling agent is used to perform an amination treatment on the porous base carrier to effectively introduce amino groups, which on the one hand improves the subsequent modification treatment effect, ensures the binding effect of the modified carrier with the antioxidant active ingredient, and improves the stability of the antioxidant active ingredient in the nylon fiber; on the other hand, it improves the compatibility and binding performance of the composite active ingredient containing the antioxidant active ingredient with nylon; then Then, in the modification step, the amino carrier is subjected to thiol modification treatment to further improve the stability and durability of the combination between the modified carrier and the antioxidant active ingredient, thereby improving its functional stability in the nylon fiber; then, in the loading step, buckwheat leaf extract and yucca extract containing antioxidant active ingredients such as flavonoids and polyphenols are selected, the buckwheat leaf extract and the yucca extract are mixed to form a loading liquid, and then the modified carrier is used for adsorption and bonding loading process to obtain a composite active ingredient; then, the composite active ingredient is used to make a functional masterbatch, which is then spun with nylon raw materials to obtain nylon large bio-fiber containing antioxidant active ingredients; the combination performance of the composite active ingredient and the nylon large bio-fiber can be effectively improved, and the nylon large bio-fiber is endowed with antioxidant and antibacterial properties, and the DPPH free radical scavenging rate and ABTS of the nylon large bio-fiber are improved. + The free radical scavenging rate and hydroxyl free radical scavenging rate both reach a high level, and the nylon biofiber has good breaking strength and breaking elongation, and good antibacterial effect; at the same time, it can also effectively avoid the problem that the antioxidant active ingredients in the plant extracts affect the subsequent dyeing. The nylon biofiber has a high dyeing percentage, and the half-dyeing time is not significantly extended compared to conventional nylon fibers. The color difference value of the dyed fiber is good, the dyeing is uniform, and the color fastness to soap washing is high; and it effectively avoids the problem that the antioxidant active ingredients in the acid dyeing process are less stable and easy to inactivate; the DPPH free radical scavenging rate and ABTS of the dyed fiber + The free radical scavenging rate, hydroxyl radical scavenging rate and antibacterial performance are not significantly different from those before dyeing; further, it can also effectively improve the water washing resistance of nylon bio-fiber, and it can still maintain good antioxidant and antibacterial properties after 20 washes.
[0154] It can be seen from Comparative Example 1 that after omitting the buckwheat leaf extract component and replacing the bisaminosilane coupling agent A-2120 with the silane coupling agent KH-550, the amination effect on the porous base carrier is reduced, which not only affects the thiol modification effect in the subsequent modification treatment, resulting in a reduction in the binding effect between the modified carrier and the antioxidant active ingredient, and a reduction in the stability of the antioxidant active ingredient in the nylon fiber, but also affects the compatibility and binding performance of the composite active ingredient with nylon. Specifically, the fiber's DPPH·free radical scavenging rate, ABTS + Significant decreases in free radical scavenging rate, hydroxyl radical scavenging rate and antibacterial performance, as well as decreases in antioxidant and antibacterial performance after 20 washes.
[0155] It can be seen from Comparative Example 2 that the use of 3A zeolite powder to replace the porous base carrier reduces the stability of the combination between the carrier and the antioxidant active ingredient; and after the amination step is omitted, the subsequent modification treatment effect is not ideal, and the combination effect of the modified carrier and the antioxidant active ingredient cannot be effectively guaranteed, and the stability of the antioxidant active ingredient in the nylon fiber is reduced; and the compatibility and binding performance of the composite active ingredient containing the antioxidant active ingredient with nylon are reduced, resulting in the antioxidant active ingredient being easily lost and ineffective during the preparation of nylon fiber and the subsequent fiber dyeing process; and the water washing resistance of nylon fiber is reduced, and the long-term antioxidant and antibacterial properties are reduced. Specifically, the fiber's DPPH·free radical scavenging rate, ABTS + The free radical scavenging rate, hydroxyl radical scavenging rate and antibacterial performance decreased, the antioxidant and antibacterial properties of the fiber decreased significantly after dyeing, and the antioxidant and antibacterial properties decreased after washing 20 times.
[0156] It can be seen from Comparative Example 3 that omitting cerium nitrate hexahydrate in the step of preparing the porous base carrier makes it impossible to further improve the active sites in the prepared porous base carrier through the synergistic coordination of the Zn / Ce bimetallic active center, resulting in a decrease in the subsequent binding stability with the antioxidant active ingredient; at the same time, after omitting the modification treatment, it is impossible to further improve the binding stability and durability of the carrier and the antioxidant active ingredient, resulting in a decrease in the functional stability of the subsequently prepared nylon fiber, and the antioxidant active ingredient is easily lost and ineffective during the preparation of the nylon fiber and the subsequent fiber dyeing process; and the water washing resistance of the nylon fiber is reduced, and the long-term antioxidant and antibacterial properties are reduced. Specifically, the fiber's DPPH·free radical scavenging rate, ABTS + The free radical scavenging rate, hydroxyl radical scavenging rate and antibacterial performance were significantly reduced, the fiber dyeing performance was reduced, and the antioxidant and antibacterial properties of the fiber after dyeing were reduced. The antioxidant and antibacterial properties of the fiber were reduced after washing 20 times.
[0157] Unless otherwise specified, all percentages used in the present invention are by mass.
[0158] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing nylon large biofiber containing antioxidant active ingredients, characterized in that: The method comprises the following steps: preparing buckwheat leaf extract, preparing yucca extract, preparing a porous base carrier, amination treatment, modification treatment, loading, preparing functional masterbatch, and spinning; The method for preparing the buckwheat leaf extract comprises: freeze-drying and crushing the buckwheat leaves, ultrasonically extracting and concentrating the buckwheat leaf extract; The method for preparing the yucca extract comprises: freeze-drying and crushing the stems and leaves of the yucca, performing ultrasonic extraction, and concentrating to obtain the yucca extract; The method for preparing the porous base carrier comprises: adding 2-methylimidazole into anhydrous methanol and dispersing it uniformly to obtain a first liquid; adding zinc nitrate hexahydrate and cerium nitrate hexahydrate into anhydrous methanol and dispersing them uniformly to obtain a second liquid; adding the second liquid into the first liquid under stirring conditions, stirring at room temperature, and standing to obtain a reaction liquid; separating to obtain a solid, and washing and drying the solid to obtain a porous base carrier; The amination treatment method comprises the following steps: putting the porous base carrier into an ethanol solution, uniformly dispersing the porous base carrier, stirring and heating the solution to 40-45° C., keeping the temperature and stirring, and dropping the bisaminosilane coupling agent A-2120; after the dropping is completed, continuing to keep the temperature and stirring, separating and obtaining a solid, washing and drying the solid, and obtaining an amination carrier; The modification treatment method comprises the following steps: adding adipoyl chloride to tetrahydrofuran, dispersing the mixture uniformly, adding the amination carrier under stirring in a nitrogen environment, stirring at room temperature for 10-12 hours, separating and obtaining a solid, washing the solid, filtering out the solid and adding the solid to N,N-dimethylformamide, adding 1,2-ethanedithiol and triethylamine under stirring in a nitrogen environment, stirring at room temperature for 5-6 hours, separating and obtaining a solid, washing and drying the solid to obtain a modified carrier; The loading method comprises mixing the buckwheat leaf extract and the yucca extract evenly to obtain a loading liquid; adding the modified carrier into the loading liquid, dispersing it evenly, stirring and heating it to 35-40° C., keeping the temperature and stirring, separating and obtaining a solid, and washing and drying the solid to obtain a composite active ingredient; The method for preparing the functional masterbatch is as follows: the composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone, and sodium stearate are put into a twin-screw extruder, the temperature is raised to 260-265° C., the temperature is maintained for melting, and then extruded and granulated to obtain the functional masterbatch; The spinning method comprises the following steps: extruding and melting nylon 66 chips and functional master batches in a temperature environment of 260-265° C., spinning, and controlling the spinning speed to be 1700-1850 m / min, and then drawing, oiling, and winding to obtain nylon large biofibers containing antioxidant active ingredients.
2. The method for preparing nylon large biofiber containing antioxidant active ingredients according to claim 1, characterized in that: In the preparation of the porous base carrier, the stirring time at room temperature after the second liquid is added to the first liquid is 50-60 minutes; the standing time is 20-30 minutes; The molar ratio of 2-methylimidazole, zinc nitrate hexahydrate and cerium nitrate hexahydrate is 2.2-2.3:0.7-0.8:0.35-0.
4.
3. The method for preparing nylon large biofiber containing antioxidant active ingredients according to claim 1, characterized in that: In the amination treatment, the volume concentration of the ethanol solution is 75-80%; Control the dropping time of bisaminosilane coupling agent A-2120 to 40-50min; After the addition of bisaminosilane coupling agent A-2120 is completed, the heat preservation and stirring time is 5-6 hours; The weight ratio of the porous base carrier, the ethanol solution and the bisaminosilane coupling agent A-2120 is 1:6-7:0.16-0.
19.
4. The method for preparing nylon large biofiber containing antioxidant active ingredients according to claim 1, characterized in that: In the modification treatment, the weight ratio of adipoyl chloride, amination carrier, 1,2-ethanedithiol, and triethylamine is 4-4.2:25-26:0.5-0.55:0.9-0.95; The weight ratio of the amination carrier to tetrahydrofuran is 1:8-9; The weight ratio of the amination carrier to N,N-dimethylformamide is 1:4-5.
5. The method for preparing nylon large biofiber containing antioxidant active ingredients according to claim 1, characterized in that: In the load, the heat preservation and stirring time after heating to 35-40°C is 5-6h; The volume ratio of buckwheat leaf extract to yucca extract was 1:1; The weight ratio of the modified carrier to the loading liquid is 1:6-6.
5.
6. The method for preparing nylon large biofiber containing antioxidant active ingredients according to claim 1, characterized in that: The method for preparing the buckwheat leaf extract comprises: freeze-drying and crushing the buckwheat leaves into buckwheat leaf powder with a particle size of 1700-1800 mesh; putting the buckwheat leaf powder into an ethanol solution with a weight of 10-12 times, performing a first ultrasonic extraction, and filtering to obtain a first extract; putting the filter residue into an ethanol solution with a weight of 8-10 times, performing a second ultrasonic extraction, and filtering to obtain a second extract; combining the first extract and the second extract, and concentrating in vacuum to 42-45% of the original volume to obtain the buckwheat leaf extract; The method for preparing the yucca extract comprises the following steps: freeze-drying and crushing the yucca stems and leaves into yucca powder with a particle size of 1700-1800 meshes; putting the yucca powder into an ethanol solution with a weight of 13-15 times, performing a first ultrasonic extraction, and filtering to obtain a first extract; putting the filter residue into an ethanol solution with a weight of 10-12 times, performing a second ultrasonic extraction, and filtering to obtain a second extract; combining the first extract and the second extract, and concentrating in vacuum to 58-60% of the original volume to obtain the yucca extract.
7. The method for preparing nylon large biofiber containing antioxidant active ingredients according to claim 6, characterized in that: In the preparation of the buckwheat leaf extract, the volume concentration of the ethanol solution used in the first ultrasonic extraction and the second ultrasonic extraction is 55-60%; the extraction temperature of the first ultrasonic extraction and the second ultrasonic extraction is 40-45° C., the ultrasonic extraction frequency is 41-43 kHz, and the ultrasonic extraction power is 200-250 W; In the preparation of the yucca extract, the volume concentration of the ethanol solution used in the first ultrasonic extraction and the second ultrasonic extraction is 55-60%; the extraction temperature of the first ultrasonic extraction and the second ultrasonic extraction is 40-45°C, the ultrasonic extraction frequency is 41-43kHz, and the ultrasonic extraction power is 200-250W.
8. The method for preparing nylon large biofiber containing antioxidant active ingredients according to claim 1, characterized in that: In the functional masterbatch, the weight ratio of the composite active ingredient, nylon 66 chips, antioxidant SEED, polyvinyl pyrrolidone and sodium stearate is 11-12:83-86:0.9-1.1:0.7-0.8:0.65-0.
75.
9. The method for preparing nylon large biofiber containing antioxidant active ingredients according to claim 1, characterized in that: In the spinning, the weight ratio of nylon 66 chips to functional masterbatch is 100:11-12.
10. A nylon biofiber containing antioxidant active ingredients, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of skin-friendly textile fabric with health care effect
CN107574489A
Synthetic fiber or filament with herbal residue and method of making same
CN108239796A
Wormwood or mint extract modified polyamide fiber and preparation method thereof
CN111235672A
Lotus leaf, radix isatidis or aloe modified polyamide fiber and preparation method thereof
CN111979592A
Macro-scale biological nylon fiber containing active ingredients of coffee and preparation method thereof
CN112981590A