BNi-2-based adhesive tape brazing filler metal and preparation method thereof

By adding silicate glass and nickel-chromium-molybdenum alloy to BNi-2 solder, an improved BNi-2-based adhesive tape solder was prepared, which solved the decline in mechanical properties of the brazed joint and the coating problem, and achieved high efficiency. The brazing process and joint performance are improved.

CN118720526APending Publication Date: 2024-10-01SUZHOU ZHONGXIN SPECIAL MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410959429.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

BNi-2 brazing filler metal contains more melt-reducing elements B, which leads to a reduction in the corrosion resistance, plasticity and strength of the brazed joint. How to accurately control the amount of brazing filler metal and the brazing filler metal in specific parts when brazing complex structures of high-temperature alloys? Coating becomes a problem.

Method used

Using BNi-2 based adhesive tape solder, adding silicate glass and nickel-chromium-molybdenum alloy, the adhesive tape solder with improved mechanical properties was prepared through ball milling, granulation, preparation of mixed slurry and casting. Solve the coating problem and improve the mechanical properties of the brazed joint.

Benefits of technology

It improves the mechanical properties of the brazed joint, simplifies the solder coating process, realizes mass production and thickness control, avoids the use of specific wire mesh or fixtures, and enhances coating efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720526A_ABST
    Figure CN118720526A_ABST
Patent Text Reader

Abstract

The invention provides BNi-2-based adhesive tape brazing filler metal and a preparation method thereof, and relates to the technical field of high-temperature alloy complex structure connection, and the BNi-2-based adhesive tape brazing filler metal comprises BNi-2 nickel-based brazing filler metal, silicate glass and nickel-chromium-molybdenum alloy. Silicate glass and nickel-chromium-molybdenum alloy are added into the BNi-2 brazing filler metal for modification, and the silicate glass is added as a strengthening phase, so that the mechanical property of a brazed joint can be improved; by adding the nickel-chromium-molybdenum alloy, diffusion of the B element in the BNi-2 brazing filler metal is promoted, generation of brittle phases is reduced, and meanwhile the mechanical property of a brazed joint can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-temperature alloy complex structure connection, and in particular to a BNi-2-based adhesive tape solder and a preparation method thereof. Background Art

[0002] BNi-2 brazing filler metal is widely used in the fields of machinery, chemical industry, aerospace, etc. due to its low melting temperature, good wettability, and the brazed joints formed have excellent antioxidant and corrosion resistance. However, because BNi-2 brazing filler metal contains a large amount of melting-reducing element B, element B is easily combined with metal elements to form a brittle phase, and local enrichment of element B is prone to melting, grain boundary penetration embrittlement and other phenomena, resulting in reduced corrosion resistance, plasticity and strength of the brazed joint, posing a microscopic hidden danger inside the brazed joint. In addition, when brazing complex structures of high-temperature alloys, how to accurately control the amount of brazing filler metal and the brazing filler metal coating at specific locations becomes an urgent problem to be solved. Summary of the invention

[0003] The problem solved by the invention is how to solve the problem of decreased joint mechanical properties caused by high content of melting-reducing element B in BNi-2 solder and inconvenient solder coating in complex structures.

[0004] In order to solve the above problems, the present invention provides a BNi-2 based adhesive tape solder and a preparation method thereof.

[0005] In a first aspect, the present invention provides a BNi-2 based adhesive tape solder, comprising a BNi-2 nickel based solder, silicate glass and a nickel-chromium-molybdenum alloy.

[0006] Optionally, based on molar parts, the brazing material comprises 80-93 parts of BNi-2 nickel-based brazing filler metal, 2-10 parts of silicate glass, and 5-15 parts of nickel-chromium-molybdenum alloy.

[0007] Optionally, the silicate glass comprises 40-60 parts by mole of SiO 2 and 10-30 parts Na 2 O.

[0008] Optionally, the silicate glass further comprises 1-3 parts of titanium dioxide in molar parts.

[0009] Second, as Figure 1 As shown, the present invention provides a method for preparing the BNi-2-based adhesive tape solder as described above, comprising the following steps:

[0010] S1: powder mixing, mixing a composite powder consisting of BNi-2 nickel-based solder, silicate glass and nickel-chromium-molybdenum alloy with a mixed solution, placing the mixture in a ball mill, and milling the mixture so that the composite powder and the mixed solution are fully mixed, the composite powder is evenly dispersed in the mixed solution, and the fully mixed composite powder and the mixed solution are dried to obtain a uniformly mixed solder powder; the solvent of the mixed solution is a mixture of chloroform and anhydrous ethanol, and the solute is triolein;

[0011] S2: Granulation: the solder powder and the binder are ball-milled at a speed of 150-300 r / min for 10-11 h, sieved and dried to obtain a bonding powder;

[0012] S3: preparing a mixed slurry, adding a plasticizer to the bonding powder, mixing evenly, and vacuum defoaming to obtain a mixed slurry;

[0013] S4: Prepare BNi-2 based adhesive tape solder, pour the mixed slurry into a tape casting machine, cast at a uniform speed to form a green billet, and dry to obtain a BNi-2 based adhesive tape solder.

[0014] Optionally, the method further includes step S0: preparation of silicate glass, which specifically includes the following steps:

[0015] S0-1: Select raw materials of silicate glass and mix them evenly, the raw materials include titanium dioxide, quartz sand, anhydrous sodium carbonate and sodium chloride, and obtain a uniformly mixed raw material powder;

[0016] S0-2: preparing glass particles, heating the raw material powder to a melting temperature, keeping the temperature, obtaining a high-temperature molten glass, and then quenching the high-temperature molten glass with water to obtain glass particles with a particle size of 0.2-5 mm;

[0017] S0-3: crushing glass particles, wet grinding the glass particles and anhydrous ethanol in a ball mill to obtain glass slurry, sieving and drying to obtain silicate glass.

[0018] Optionally, in step S0-2, the raw material powder is heated at a rate of 7-10°C / min, the melting temperature is 900°C-1200°C, and the insulation time is 50-90min.

[0019] Optionally, in step S0-3, the mass ratio of anhydrous ethanol to glass particles is (1-1.2):1.

[0020] Optionally, in step S2, the mass ratio of solder powder to adhesive is 1:(0.7-1), the solvent of the adhesive is acetone, the solute is polymethyl methacrylate, and the mass of the solute accounts for 2%-4% of the mass of the solvent.

[0021] Optionally, in step S4, the green blank is dried at 120-140° C. for 7-9 hours, and the thickness of the obtained BNi-2-based adhesive tape solder is 40-200 μm.

[0022] The beneficial effects of the BNi-2-based adhesive tape solder and the preparation method thereof of the present invention are:

[0023] Silicate glass and nickel-chromium-molybdenum alloy are added to the BNi-2 brazing filler metal for modification. The addition of silicate glass as a strengthening phase can improve the mechanical properties of the brazed joint; the addition of nickel-chromium-molybdenum alloy is beneficial to promoting the diffusion of element B in the BNi-2 brazing filler metal, further diluting the element B in the brazing filler metal layer, reducing the formation of brittle phases, and also improving the mechanical properties of the brazed joint.

[0024] BNi-2-based adhesive tape solder solves the problem of solder coating in the process of complex structure connection: compared with screen printing technology, BNi-2-based adhesive tape solder does not require a specific screen; the preparation of block solder in the past required remelting, rolling and cutting, and the production process was relatively complicated. BNi-2-based adhesive tape solder can be mass-produced, and the thickness of the solder can be controlled. In the process of solder coating and brazing of complex structures, there is no need to use a specific fixture, and it can be used after sticking. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Flow chart of the preparation method of the BNi-2 based adhesive tape solder of this embodiment. DETAILED DESCRIPTION

[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0027] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;

[0028] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0029] In view of the problems existing in the above-mentioned related technologies, this embodiment provides a BNi-2-based adhesive tape solder and a preparation method thereof.

[0030] The present embodiment provides a BNi-2 based adhesive tape solder, comprising a BNi-2 nickel based solder, silicate glass and a nickel-chromium-molybdenum alloy.

[0031] Silicate glass and nickel-chromium-molybdenum alloy are added to the BNi-2 brazing filler metal for modification. The addition of silicate glass as a strengthening phase can improve the mechanical properties of the brazed joint; the addition of nickel-chromium-molybdenum alloy is beneficial to promoting the diffusion of the B element in the BNi-2 brazing filler metal, reducing the formation of the brittle phase, and also improving the mechanical properties of the brazed joint.

[0032] BNi-2-based adhesive tape solder solves the problem of solder coating in the process of complex structure connection: compared with screen printing technology, BNi-2-based adhesive tape solder does not require a specific screen; the preparation of block solder in the past required remelting, rolling and cutting, and the production process was relatively complicated. BNi-2-based adhesive tape solder can be mass-produced, and the thickness of the solder can be controlled. In the process of solder coating and brazing of complex structures, there is no need to use a specific fixture, and it can be used after sticking.

[0033] Optionally, based on molar parts, the brazing material comprises 80-93 parts of BNi-2 nickel-based brazing filler metal, 2-10 parts of silicate glass, and 5-15 parts of nickel-chromium-molybdenum alloy.

[0034] Specifically, the nickel-chromium-molybdenum alloy may be GH536 alloy, which is a high-temperature alloy, a nickel-chromium-molybdenum alloy with cobalt and tungsten added, and has the function of resisting carburizing and nitriding atmospheres.

[0035] Optionally, the silicate glass comprises 40-60 parts by mole of SiO2 and 10-30 parts Na 2 O.

[0036] Specifically, the raw materials include quartz sand, anhydrous sodium carbonate and sodium chloride, wherein the quartz sand introduces SiO 2 , anhydrous sodium carbonate introduces Na 2 O, sodium chloride as high temperature clarifier.

[0037] Optionally, the silicate glass further comprises 1-3 parts of titanium dioxide in molar parts.

[0038] In this optional embodiment, a small amount of titanium dioxide is added to obtain titanium-doped silicate glass. The Ti element improves the overall performance of the brazed joint by affecting the solidification process, mechanical properties and surface properties of the nickel alloy brazing material.

[0039] This embodiment provides a method for preparing the BNi-2-based adhesive tape solder as described above, comprising the following steps:

[0040] S1: powder mixing, mixing a composite powder consisting of BNi-2 nickel-based solder, silicate glass and nickel-chromium-molybdenum alloy with a mixed solution, placing the mixture in a ball mill, and milling the mixture so that the composite powder and the mixed solution are fully mixed, the composite powder is evenly dispersed in the mixed solution, and the fully mixed composite powder and the mixed solution are dried to obtain a uniformly mixed solder powder; the solvent of the mixed solution is a mixture of chloroform and anhydrous ethanol, and the solute is triolein;

[0041] S2: Granulation: the solder powder and the binder are ball-milled at a speed of 150-300 r / min for 10-11 h, sieved and dried to obtain a bonding powder;

[0042] S3: preparing a mixed slurry, adding a plasticizer to the bonding powder, mixing evenly, and vacuum defoaming to obtain a mixed slurry;

[0043] S4: Prepare BNi-2 based adhesive tape solder, pour the mixed slurry into a tape casting machine, cast at a uniform speed to form a green billet, and dry to obtain a BNi-2 based adhesive tape solder.

[0044] Specifically, S1: powder mixing, mixing a composite powder consisting of BNi-2 nickel-based solder, silicate glass and nickel-chromium-molybdenum alloy with a mixed solution, placing the mixture in a ball mill, and ball milling at a speed of 150-300 r / min for 10-12 hours to fully mix the composite powder with the mixed solution, and uniformly disperse the composite powder in the mixed solution, then taking out the grinding balls, placing the ball mill in a drying oven, drying the fully mixed composite powder and the mixed solution, and drying at 50° C. for 3-5 hours to obtain a uniformly mixed solder powder;

[0045] The solvent of the mixed solution is a mixture of chloroform and anhydrous ethanol, the mass ratio of chloroform to anhydrous ethanol is 1:(0.2-0.3), the solute is triolein, and the mass of the solute accounts for 4%-5% of the mass of the solvent;

[0046] S2: Granulation, solder powder and binder are added to a ball mill, wherein the mass ratio of solder powder to binder is 1:(0.8-1), and ball milled at a speed of 150-300r / min for 10-11h to fully mix the solder powder and binder. After taking out the grinding balls, the slurry is filtered through a 300-mesh sieve to remove large particles and undissolved organic matter. The filtered slurry is placed in a culture dish and dried at 50°C for 3h to obtain bonding powder;

[0047] The adhesive solvent is acetone, the solute is polymethyl methacrylate, and the mass of the solute accounts for 2%-4% of the mass of the solvent;

[0048] S3: preparing a mixed slurry, adding a plasticizer to the bonding powder, mixing the bonding powder and the plasticizer at a mass ratio of 1:(0.2-0.4) to prepare a slurry with a certain fluidity, and then magnetically stirring for 50-70 minutes to mix evenly, putting the slurry into a vacuum defoaming machine for 35-45 minutes, vacuum defoaming, and obtaining a uniform mixed slurry of BNi-2-based adhesive tape solder;

[0049] The plasticizer is a mixture of terpineol and dibutyl phthalate, and the mass ratio of terpineol to dibutyl phthalate is 1:(0.3-0.5);

[0050] S4: preparing a BNi-2-based adhesive tape solder, setting the scraper height of the tape casting machine, pouring the mixed slurry into the tape casting machine, casting at a uniform speed to form a green blank, and then drying the green blank at 120-150° C. for 7-9 hours to remove the moisture and some organic matter in the slurry, and then peeling it off from the base tape to obtain a BNi-2-based adhesive tape solder;

[0051] The thickness of BNi-2 based adhesive tape solder is 40-200μm.

[0052] In this embodiment, the composition powder and anhydrous ethanol are wet-milled in a ball mill and the solvent is dried to make the composition powder uniformly dispersed. The solder powder and the adhesive are ball-milled and the solvent is dried to make the bonding powder uniformly dispersed and the bonding powders are densely bonded, thereby improving the density of the solder. The plasticizer plays the role of both a plasticizer and a solvent, further improving the solid content of the BNi-2-based adhesive tape solder. The mixed slurry can be cast by casting according to different weld width requirements to produce a BNi-2-based adhesive tape solder with a certain thickness and uniform composition, uniform thickness, certain mechanical strength, good plasticity, and ductility, which can more accurately control the weld width. The casting method can be continuously operated, has a high degree of automation, mature technology, and can be mass-produced, effectively improving the coating efficiency.

[0053] Optionally, the method further includes step S0: preparation of silicate glass, which specifically includes the following steps:

[0054] S0-1: Select raw materials of silicate glass and mix them evenly, the raw materials include titanium dioxide, quartz sand, anhydrous sodium carbonate and sodium chloride, and obtain a uniformly mixed raw material powder;

[0055] S0-2: preparing glass particles, heating the raw material powder to a melting temperature, keeping the temperature, obtaining a high-temperature molten glass, and then quenching the high-temperature molten glass with water to obtain glass particles with a particle size of 0.2-5 mm;

[0056] S0-3: crushing glass particles, wet grinding the glass particles and anhydrous ethanol in a ball mill to obtain glass slurry, sieving and drying to obtain silicate glass.

[0057] Specifically, S0-1: select raw material powder of silicate glass according to a certain ratio and add it into a crucible, mix it evenly, and obtain a uniformly mixed raw material powder; the raw materials include titanium dioxide, quartz sand, anhydrous sodium carbonate and sodium chloride, titanium dioxide introduces Ti element, quartz sand introduces SiO 2 , anhydrous sodium carbonate introduces Na 2 O, sodium chloride is used as a high-temperature clarifier, the specific molar ratio is 1-3 parts of titanium dioxide, 20-45 parts of quartz sand, 10-20 parts of anhydrous sodium carbonate, and an average of 0.3g of sodium chloride is added to every 100g of powder;

[0058] S0-2: Prepare glass particles. Heat the raw material powder in a muffle furnace at a certain rate of 7-10°C / min. When the melting temperature reaches 900°C-1200°C, keep the temperature for 50-90min to melt, homogenize and clarify the glass. Then quickly pour the high-temperature molten glass into cold water for water quenching to obtain glass particles with a particle size of 0.2-5mm.

[0059] S0-3: crushing glass particles, putting the glass particles into a mortar and crushing them, and then placing them in a ball mill, at a speed of 500-600r / min, adding grinding balls at a mass ratio of grinding balls to glass particles of (35-45):1, dry grinding for 1-2h, and then adding anhydrous ethanol at a mass ratio of anhydrous ethanol to glass particles of (1-1.5):1, at a speed of 500-00r / min, stop for 4min after each ball milling for 10min, wet grinding for a total of 10-12h, taking out the grinding balls to obtain glass powder slurry, filtering the glass powder slurry through a 500-mesh sieve, and drying at 50°C for 10h to obtain silicate glass.

[0060] In this optional embodiment, titanium dioxide introduces Ti element, and quartz sand introduces SiO 2 , anhydrous sodium carbonate introduces Na 2 O, sodium chloride as a high temperature clarifier. A small amount of Ti element is added to obtain titanium-doped silicate glass. The Ti element improves the comprehensive performance of the brazed joint by affecting the solidification process, mechanical properties and surface properties of the nickel alloy brazing filler metal.

[0061] Optionally, in step S0-2, the raw material powder is heated at a rate of 7-10°C / min, the melting temperature is 900°C-1200°C, and the insulation time is 50-90min.

[0062] Optionally, in step S0-3, the mass ratio of anhydrous ethanol to glass particles is (1-1.2):1.

[0063] Optionally, in step S2, the mass ratio of solder powder to adhesive is 1:(0.7-1), the solvent of the adhesive is acetone, the solute is polymethyl methacrylate, and the mass of the solute accounts for 2%-4% of the mass of the solvent.

[0064] Optionally, in step S4, the green blank is dried at 120-140° C. for 7-9 hours, and the thickness of the obtained BNi-2-based adhesive tape solder is 40-200 μm.

[0065] The present invention is further described below in conjunction with specific embodiments.

[0066] Example 1

[0067] The preparation method of BNi-2 based adhesive tape solder is specifically carried out according to the following steps:

[0068] 1. Silicate glass, measured by mole, is composed of 40 parts of SiO 2 and 30 parts Na 2 O composition;

[0069] 2. Add the raw material powder into the crucible, mix evenly, heat at a certain rate in a muffle furnace, and when the melting temperature is reached, keep it warm for a period of time to melt, homogenize and clarify the glass, and then quickly pour the high-temperature molten glass into cold water for water quenching to obtain glass particles with a particle size of 5 mm. Put the glass particles into a mortar and crush them, then place them in a ball ink tank, add grinding balls at a ratio of 35:1 to the mass ratio of grinding balls to glass particles at a speed of 600r / min, dry grind for 1h, then add solvent at a ratio of 1:1 to the mass ratio of solvent to glass particles, wet grind for 2h at a speed of 400r / min to obtain glass powder slurry, filter the glass powder slurry through a 325-mesh screen, and dry it at 50°C for 12h to obtain glass powder with a particle size of less than 45μm;

[0070] 3. Take 80 parts of BNi-2, 2 parts of silicate glass, and 10 parts of GH536 by mole percentage;

[0071] Fourth, mix the solder powder and the solvent in a mass ratio of 1:0.75 and place them in a ball mill, then add a small amount of dispersant, the mass of the dispersant is 4% of the mass of the solder powder, and ball mill at a speed of 200r / min for 24 hours to evenly disperse the solder powder in the solvent to obtain a first-time ball milling mixed slurry. Add a binder and a plasticizer to the first-time ball milling mixed slurry, wherein the ratio of the binder to the plasticizer is 1:1, and the total mass of the two is 20% of the solder powder, and continue to ball mill at a speed of 200r / min for 24 hours to obtain a slurry with uniform composition, put the slurry into a vacuum degassing machine for 30 minutes to remove the bubbles, and then filter it through a 200-mesh screen to remove large particles of residue and undissolved organic matter to obtain a uniform solder powder mixed slurry;

[0072] 5. Set the scraper height of the tape casting machine, pour the prepared mixed slurry into the tape casting machine, cast at a uniform speed to form a green blank, then dry the green blank at 40 degrees for 24 hours, peel it off from the base tape, and obtain a 100μm thick solder adhesive tape;

[0073] 6. The prepared BNi-2 based adhesive tape brazing filler metal was used for brazing of GH3536 high temperature alloy, and the maximum shear strength at room temperature was measured to be 140.5 MPa.

[0074] Example 2

[0075] The preparation method of BNi-2 based adhesive tape solder is specifically carried out according to the following steps:

[0076] 1. Silicate glass, measured by mole, is composed of 40 parts of SiO 2 , 30 parts Na 2 O and 3 parts TiO 2 composition;

[0077] 2. Add the raw material powder into the crucible, mix evenly, heat at a certain rate in a muffle furnace, and when the melting temperature is reached, keep it warm for a period of time to melt, homogenize and clarify the glass, and then quickly pour the high-temperature molten glass into cold water for water quenching to obtain glass particles with a particle size of 1 mm. Put the glass particles into a mortar and crush them, then place them in a ball ink tank, add grinding balls at a ratio of 45:1 to the mass ratio of grinding balls to glass particles at a speed of 600r / min, dry grind for 1h, then add solvent at a ratio of 1.5:1 to the mass ratio of solvent to glass particles, wet grind for 2h at a speed of 400r / min to obtain glass powder slurry, filter the glass powder slurry through a 325-mesh screen, and dry it at 50°C for 12h to obtain glass powder with a particle size of less than 45μm;

[0078] c. Take 80 parts of BNi-2, 2 parts of Ti-containing silicate glass, and 10 parts of GH536 by mole percentage;

[0079] d. Mix the solder powder and the solvent in a mass ratio of 1:0.8 and place them in a ball mill. Add a small amount of dispersant, the mass of which is 5% of the mass of the solder powder. Mill at a speed of 200 r / min for 24 hours to evenly disperse the solder powder in the solvent to obtain a first-time ball milling mixed slurry. Add a binder and a plasticizer to the first-time ball milling mixed slurry, wherein the ratio of the binder to the plasticizer is 1:1, and the total mass of the two is 20% of the solder powder. Continue to ball mill at a speed of 200 r / min for 24 hours to obtain a slurry with uniform composition. Put the slurry into a vacuum degassing machine and run it for 40 minutes to remove the bubbles. Then filter it through a 200-mesh screen to remove large particle residues and undissolved organic matter to obtain a uniform solder powder mixed slurry.

[0080] e. Set the scraper height of the tape casting machine, pour the prepared mixed slurry into the tape casting machine, cast at a uniform speed to form a green blank, then dry the green blank at 50°C for 24 hours, peel it off from the base tape, and obtain a 100μm thick solder adhesive tape;

[0081] f. The prepared BNi-2 based adhesive tape brazing filler metal was used for brazing of GH3536 high temperature alloy, and the maximum shear strength at room temperature was measured to be 167.5 MPa.

[0082] Comparative Example 1

[0083] The preparation method of BNi-2 based adhesive tape solder is specifically carried out according to the following steps:

[0084] 1. Silicate glass, measured by mole, is composed of 40 parts of SiO 2 and 30 parts Na 2 O composition;

[0085] 2. Add the raw material powder into the crucible, mix evenly, heat at a certain rate in a muffle furnace, and when the melting temperature is reached, keep it warm for a period of time to melt, homogenize and clarify the glass, and then quickly pour the high-temperature molten glass into cold water for water quenching to obtain glass particles with a particle size of 5 mm. Put the glass particles into a mortar and crush them, then place them in a ball ink tank, add grinding balls at a ratio of 35:1 to the mass ratio of grinding balls to glass particles at a speed of 600r / min, dry grind for 1h, then add solvent at a ratio of 1:1 to the mass ratio of solvent to glass particles, wet grind for 2h at a speed of 400r / min to obtain glass powder slurry, filter the glass powder slurry through a 325-mesh screen, and dry it at 50°C for 12h to obtain glass powder with a particle size of less than 45μm;

[0086] 3. Take 80 parts of BNi-2 and 3 parts of silicate glass by mole percentage;

[0087] Fourth, mix the solder powder and the solvent in a mass ratio of 1:0.75 and place them in a ball mill, then add a small amount of dispersant, the mass of the dispersant is 4% of the mass of the solder powder, and ball mill at a speed of 200r / min for 24 hours to evenly disperse the solder powder in the solvent to obtain a first-time ball milling mixed slurry. Add a binder and a plasticizer to the first-time ball milling mixed slurry, wherein the ratio of the binder to the plasticizer is 1:1, and the total mass of the two is 20% of the solder powder, and continue to ball mill at a speed of 200r / min for 24 hours to obtain a slurry with uniform composition, put the slurry into a vacuum degassing machine for 30 minutes to remove the bubbles, and then filter it through a 200-mesh screen to remove large particles of residue and undissolved organic matter to obtain a uniform solder powder mixed slurry;

[0088] 5. Set the scraper height of the tape casting machine, pour the prepared mixed slurry into the tape casting machine, cast at a uniform speed to form a green blank, then dry the green blank at 40 degrees for 24 hours, peel it off from the base tape, and obtain a 100μm thick solder adhesive tape;

[0089] 6. The prepared BNi-2 based adhesive tape brazing filler metal was used for brazing of GH3536 high temperature alloy, and the maximum shear strength at room temperature was measured to be 110.8 MPa.

[0090] Comparative Example 2

[0091] The preparation method of BNi-2 based adhesive tape solder is specifically carried out according to the following steps:

[0092] 1. Take 80 parts of BNi-2 and 10 parts of GH536 by mole percentage;

[0093] 2. Mix the solder powder and the solvent in a mass ratio of 1:0.75 and place them in a ball mill. Add a small amount of dispersant, the mass of which is 4% of the mass of the solder powder. Mill at a speed of 200 r / min for 24 hours to evenly disperse the solder powder in the solvent to obtain a first-time ball-milled mixed slurry. Add a binder and a plasticizer to the first-time ball-milled mixed slurry, wherein the ratio of the binder to the plasticizer is 1:1, and the total mass of the two is 20% of the solder powder. Continue to ball mill at a speed of 200 r / min for 24 hours to obtain a slurry with uniform composition. Put the slurry into a vacuum degassing machine and run it for 30 minutes to remove the bubbles. Then filter it through a 200-mesh screen to remove large particle residues and undissolved organic matter to obtain a uniform solder powder mixed slurry.

[0094] 3. Set the scraper height of the tape casting machine, pour the prepared mixed slurry into the tape casting machine, cast at a uniform speed to form a green blank, then dry the green blank at 40 degrees for 24 hours, peel it off from the base tape, and obtain a 100μm thick solder adhesive tape;

[0095] 4. The prepared BNi-2 based adhesive tape brazing filler metal was used for brazing of GH3536 high temperature alloy, and the maximum shear strength at room temperature was measured to be 122.6 MPa.

[0096] Comparative Example 3

[0097] GH3536 nickel-based high-temperature alloy was directly brazed using BNi-2 metal foil, and the maximum shear strength at room temperature was measured to be 106.8 MPa.

[0098] Silicate glass and nickel-chromium-molybdenum alloy are added to the BNi-2 brazing filler metal for synergistic modification. The addition of silicate glass as a strengthening phase can improve the mechanical properties of the brazed joint and the shear strength of the welded joint; the addition of nickel-chromium-molybdenum alloy is beneficial to promoting the diffusion of the B element in the BNi-2 brazing filler metal, further diluting the boron element in the brazing filler metal layer, reducing the formation of the brittle phase, and also improving the mechanical properties of the brazed joint and the shear strength of the welded joint.

[0099] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A BNi-2 based adhesive tape solder, characterized in that: Including BNi-2 nickel-based brazing filler metal, silicate glass and nickel-chromium-molybdenum alloy.

2. The BNi-2 based adhesive tape solder according to claim 1, characterized in that: The invention comprises, by mole, 80-93 parts of BNi-2 nickel-based solder, 2-10 parts of silicate glass, and 5-15 parts of nickel-chromium-molybdenum alloy.

3. The BNi-2 based adhesive tape solder according to claim 1, characterized in that: In terms of molar parts, the silicate glass includes 40-60 parts of SiO2 and 10-30 parts of Na2O.

4. The BNi-2 based adhesive tape solder according to claim 3, characterized in that: The silicate glass further comprises 1-3 parts of titanium dioxide in terms of molar parts.

5. A method for preparing the BNi-2 based adhesive tape solder as claimed in claim 1 or 2, characterized in that: The following steps are involved: S1: powder mixing, mixing a composite powder consisting of BNi-2 nickel-based solder, silicate glass and nickel-chromium-molybdenum alloy with a mixed solution, placing the mixture in a ball mill, and milling the mixture to fully mix the composite powder with the mixed solution. The composite powder is evenly dispersed in the mixed solution, and the fully mixed composite powder and the mixed solution are dried to obtain a uniformly mixed solder powder; the solvent of the mixed solution is a mixture of chloroform and anhydrous ethanol, and the solute is triolein; S2: Granulation, the solder powder and the binder are ball-milled at a speed of 150-300 r / min for 10-11 h, sieved and then dried to obtain a bonding powder; S3: preparing a mixed slurry, adding a plasticizer to the bonding powder, mixing evenly, and vacuum defoaming to obtain a mixed slurry; S4: preparing a BNi-2-based adhesive tape solder, pouring the mixed slurry into a tape casting machine, casting at a uniform speed to form a green billet, and drying to obtain a BNi-2-based adhesive tape solder.

6. A method for preparing the BNi-2 based adhesive tape solder as claimed in claim 5, characterized in that: The method further comprises step S0: preparation of silicate glass, which specifically comprises the following steps: S0-1: Selecting raw materials of the silicate glass and mixing them uniformly, the raw materials include titanium dioxide, quartz sand, anhydrous sodium carbonate and sodium chloride to obtain uniformly mixed raw material powder; S0-2: preparing glass particles, heating the raw material powder to a melting temperature, keeping the temperature, obtaining a high-temperature molten glass, and then quenching the high-temperature molten glass with water to obtain glass particles with a particle size of 0.2-5 mm; S0-3: crushing the glass particles, wet-grinding the glass particles with anhydrous ethanol in a ball mill to obtain glass slurry, sieving and drying to obtain the silicate glass.

7. The method for preparing the BNi-2 based adhesive tape solder according to claim 6, characterized in that: In step S0-2, the raw material powder is heated at a rate of 7-10°C / min, the smelting temperature is 900°C-1200°C, and the holding time is 50-90min.

8. The method for preparing the BNi-2 based adhesive tape solder according to claim 6, characterized in that: In step S0-3, the mass ratio of anhydrous ethanol to the glass particles is (1-1.2):

1.

9. The method for preparing the BNi-2 based adhesive tape solder according to claim 5, characterized in that: In step S2, the mass ratio of the solder powder to the adhesive is 1:(0.7-1), the solvent of the adhesive is acetone, the solute is polymethyl methacrylate, and the mass of the solute accounts for 2%-4% of the mass of the solvent.