Method for judging bubble source in glass substrate and method for eliminating retained bubbles in glass substrate

By counting changes in the number of bubbles and specific stirring processes in the production of glass substrates, the trapped bubbles in the platinum channel mixing barrel can be accurately judged and eliminated, which solves the problem of difficulty in judging and eliminating trapped bubbles in the production of glass substrates, and improves the glass yield rate and Production efficiency.

CN118724428AActive Publication Date: 2024-10-01WUHU TUNGHSU PHOTOELECTRIC SCI & TECHCO +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410999258.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

In the production of glass substrates, especially ultra-thin glass substrates, it is difficult to accurately judge and quickly eliminate trapped air bubbles in the platinum channel mixing barrel, resulting in reduced glass yield and low production efficiency.

Method used

In the production of glass substrates, stop the stirring rod rotation timing, count the changes in the number of bubbles, determine the bubble type according to specific conditions, and adopt a stirring cycle of forward rotation, stop rotation, reverse rotation, and stop rotation, and repeat the process to discharge the trapped bubbles. Ensure that the glass liquid continues to flow and gradually eliminate bubbles in the stagnant layer.

Benefits of technology

It can quickly and accurately determine the type of bubbles, effectively reduce or eliminate trapped bubbles, improve the yield and production efficiency of glass substrates, and avoid long-term trial and error and misjudgment in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724428A_ABST
    Figure CN118724428A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of glass substrate manufacturing, and discloses a method for judging the source of bubbles in a glass substrate and a method for eliminating remaining bubbles in the glass substrate, and the method comprises the following steps: in the process of preparing the glass substrate by a continuous method, the number of bubbles with the diameter of 1-10mm in the glass substrate accounts for more than 80%; the number x of bubbles of a single glass substrate is greater than or equal to 2 / plate; stopping rotating the stirring rod in the platinum channel stirring barrel, observing the change rule of the number of single-plate bubbles in the glass substrate after the stirring rod stops rotating and the stirring rod is restarted, and judging the type of the bubbles in the glass substrate. The method is systematic, whether the bubbles are the bubbles retained in the stirring barrel or not can be judged in a short time, the retained bubbles are rapidly reduced and eliminated, and the glass yield is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass substrate manufacturing, and in particular to a method for determining the source of bubbles in a glass substrate and a method for eliminating trapped bubbles in a glass substrate. Background Art

[0002] In the production of optoelectronic display glass substrates, such as OLED (organic light-emitting semiconductor) and LTPS (low-temperature polycrystalline silicon) glass substrates, as well as ultra-thin glass substrates with a thickness of less than 0.1mm, the glass mixture is first put into the kiln for high-temperature melting through the overflow down-draw method, and after being stirred and clarified by the platinum channel, it flows into the molding furnace body and overflows through the overflow brick to form a glass ribbon, and then cut into semi-finished products. Ultra-thin flexible glass has the characteristics of good bendability, good transparency, heat resistance and stability, high hardness, but it is more difficult to produce. Glass substrates, especially ultra-thin glass substrates, have higher requirements for bubble defects, the platinum channel body is longer, the clarification process is more complicated, and it is easier to produce clarified bubbles. Bubbles are a common internal defect, and there are many reasons for their generation, which can be divided into three types: entrained bubbles, clarified bubbles and retained bubbles. Entrained bubbles are generated by external air being entrained in the glass liquid, and clarified bubbles are generated from the inside. The generation mechanism and adjustment direction of each bubble are quite different. The platinum channel stirring barrel and stirring rod are very important equipment, which plays an important role in homogenizing the glass liquid and eliminating streak defects. There is a slow-flowing glass retention layer on the top of the mixing barrel, which is easy to retain bubbles. Especially in the early stage of production line production, when the liquid level is established and the auxiliary heater on the top of the mixing barrel is abnormally shut down, it is very easy to generate and retain bubbles. This type of bubble is generally very similar to clarified bubbles. It is very easy to misjudge based on experience, resulting in poor countermeasures and seriously affecting the production efficiency of the production line.

[0003] In the existing technology, engineers adjust the process based on their own experience, and then determine the location and cause of the bubbles according to the changes in the bubbles and formulate corresponding countermeasures. This requires a very high level of experience from engineers, a long trial and error time, a long countermeasure cycle and is very prone to misjudgment, resulting in the wrong countermeasure direction, which seriously affects the glass yield.

[0004] Therefore, it is urgent to develop a method for accurately judging and quickly reducing or eliminating trapped bubbles in the mixing barrel to improve the glass yield. Summary of the invention

[0005] The purpose of the present invention is to provide a method for accurately judging and quickly reducing or eliminating trapped bubbles in a mixing barrel.

[0006] In order to achieve the above object, a first aspect of the present invention provides a method for determining the type of bubbles in a glass substrate prepared by a continuous process, the method comprising:

[0007] (1) In a process of preparing a glass substrate by a continuous method, a glass liquid is introduced into a platinum channel stirring barrel with a stirring rod for stirring, and a material obtained after the stirring is subjected to a molding process to obtain a product glass substrate;

[0008] (2) When the product glass substrate is a defective product, the stirring rod in the platinum channel stirring barrel is stopped and the timing is started as t0;

[0009] (3) counting the number of bubbles in the single plate of the product glass substrate obtained from time t1 to time t2, and if it is found that the number of bubbles in the single plate of the product glass substrate meets condition (a1) or condition (b1) as time goes by, re-rotating the stirring rod in the platinum channel stirring barrel;

[0010] (a1) Condition: The number of bubbles in a single plate of the obtained product glass substrate increases first and then decreases to x±3 / plate, and remains stable at x±3 / plate;

[0011] (b1) Condition: The number of bubbles in a single plate of the obtained product glass substrate increases first and then decreases to ≤0.5 / plate, and remains stable at ≤0.5 / plate;

[0012] (4) counting the number of bubbles in a single plate of the product glass substrate obtained from time t2 to time t3, and if it is found that as time passes, in the process that satisfies condition (a1) in step (3), the number of bubbles in a single plate of the product glass substrate meets condition (a2), then the bubbles in the product glass substrate are determined to be clear bubbles; if it is found that as time passes, in the process that satisfies condition (b1) in step (3), the number of bubbles in a single plate of the product glass substrate meets condition (b2), then the bubbles in the product glass substrate are determined to be retained bubbles;

[0013] (a2) Condition: The number of bubbles in a single plate of the obtained product glass substrate remains stable at x ± 3 per plate;

[0014] (b2) Condition: The number of bubbles in the single plate of the obtained product glass substrate remains stable at ≤0.5 / plate;

[0015] t0=0h; t1 is 1.5h-5h; t2 is at least 2h greater than t1; t3 is at least 2h greater than t2;

[0016] The ratio K of the number of bubbles with a diameter of 1-10 mm in any one of the obtained product glass substrates to the total number of bubbles in the product glass substrate is defined, and the number of bubbles in a single plate is x; in steps (3) and (4), K of the product glass substrate is ≥80%, and x is ≥2.

[0017] A second aspect of the present invention provides a method for eliminating trapped bubbles in a glass substrate, the method comprising:

[0018] S1: Keeping the glass liquid flowing continuously, lifting the stirring rod (2) in the platinum channel stirring barrel (1) into the retention layer (5) containing retained bubbles without penetrating the retention layer (5);

[0019] S2: starting the stirring rod (2) and stirring in the order of forward rotation, stop I, reverse rotation, and stop II as one stirring cycle; repeating the stirring cycle 0-5 times, so that the retained bubbles in the retention layer (5) enter the glass liquid in the stirring barrel (1);

[0020] S3: Stop rotating the stirring rod (2) to remove bubbles; the stirring rod (2) is stopped for more than 15 hours.

[0021] The process method of the present invention can solve the problem of trapped bubbles in the platinum channel stirring barrel caused by heating of the production line and damage to the equipment during normal production.

[0022] The method provided by the present invention can quickly discharge bubbles in the retention layer in a short time, thereby preventing bubbles in the retention layer from intermittently flowing into the glass liquid, causing glass plates to be rejected for a long time and in large quantities, thereby improving the glass yield and production efficiency.

[0023] Compared with the traditional tentative defoaming countermeasures, the present invention is a systematic method that can determine in a short time whether the bubbles are bubbles retained in the mixing barrel and quickly reduce and eliminate them, thereby improving the glass yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of the platinum channel mixing barrel.

[0025] Description of Reference Numerals

[0026] 1- stirring barrel, 2- stirring rod, 3- liquid level line, 4- auxiliary heating device, 5- retention layer DETAILED DESCRIPTION

[0027] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0028] The "I" or "II" in "Stop I, Stop II" described in the present invention has no practical meaning and is only used to distinguish process flows with the same description.

[0029] The "defective product" in the present invention refers to a glass substrate product that cannot meet the product quality standard or application requirements. Those skilled in the art can distinguish good products from defective products according to different production quality requirements. In the present invention, the defective product is preferably a glass substrate with a single plate bubble number ≥ 2 / plate or a plate surface bubble size ≥ 0.2 mm.

[0030] The method of the present invention can solve the problem of trapped bubbles in the platinum channel stirring barrel caused by heating of the production line and damage to the equipment during normal production.

[0031] like Figure 1 As shown, the platinum channel needs to establish an initial glass liquid level in the channel at the initial stage of heating up the production line. If the clarification process of the furnace channel fails to meet the requirement of eliminating clarified bubbles during the process, the clarified bubbles in the liquid level establishment process will be retained in the retention layer 5 on the upper part of the stirring barrel 1 to form retained bubbles that are difficult to remove. The glass liquid in the retention layer flows slowly, and then is slowly brought into the stirring barrel as the stirring rod 2 rotates. As the glass liquid flows out, bubble defects are formed, and retained bubbles in the stirring barrel appear.

[0032] During the production process of the production line, the auxiliary heating device 4 in the upper space of the mixing barrel is abnormally shut down (in an ultra-high temperature environment, electrical components may be damaged), causing the temperature of the upper space of the mixing barrel and the temperature of the glass liquid on the surface of the liquid to drop below the normal production temperature, causing the clarified bubbles at the bottom to enter the retention layer at the top of the mixing barrel to form retained bubbles, which are then slowly brought into the mixing barrel 1 as the stirring rod 2 rotates. As the glass liquid flows out, bubble defects are formed, and retained bubbles appear in the mixing barrel.

[0033] The size of trapped bubbles is very similar to that of clarified bubbles, but the causes and locations are different. If the trapped bubbles are treated as clarified bubbles, the effect will be small and the yield rate will be affected. The general defoaming countermeasure method is to repeatedly adjust the process parameters to verify the source of the bubbles and then take targeted countermeasures. This countermeasure cycle will be relatively long and cause great damage to the process stability.

[0034] In order to solve the above problems, the method directly determines the source and cause of the bubbles through simple verification actions, and then solves the retained bubbles in the mixing barrel through targeted process adjustments.

[0035] As mentioned above, the first aspect of the present invention provides a method for determining the type of bubbles in a glass substrate prepared by a continuous process, the method comprising:

[0036] (1) In a process of preparing a glass substrate by a continuous method, a glass liquid is introduced into a platinum channel stirring barrel with a stirring rod for stirring, and a material obtained after the stirring is subjected to a molding process to obtain a product glass substrate;

[0037] (2) When the product glass substrate is a defective product, the stirring rod in the platinum channel stirring barrel is stopped and the timing is started as t0;

[0038] (3) counting the number of bubbles in the single plate of the product glass substrate obtained from time t1 to time t2, and if it is found that the number of bubbles in the single plate of the product glass substrate meets condition (a1) or condition (b1) as time goes by, re-rotating the stirring rod in the platinum channel stirring barrel;

[0039] (a1) Condition: The number of bubbles in a single plate of the obtained product glass substrate increases first and then decreases to x±3 / plate, and remains stable at x±3 / plate;

[0040] (b1) Condition: The number of bubbles in a single plate of the obtained product glass substrate increases first and then decreases to ≤0.5 / plate, and remains stable at ≤0.5 / plate;

[0041] (4) counting the number of bubbles in a single plate of the product glass substrate obtained from time t2 to time t3, and if it is found that as time passes, in the process that satisfies condition (a1) in step (3), the number of bubbles in a single plate of the product glass substrate meets condition (a2), then the bubbles in the product glass substrate are determined to be clear bubbles; if it is found that as time passes, in the process that satisfies condition (b1) in step (3), the number of bubbles in a single plate of the product glass substrate meets condition (b2), then the bubbles in the product glass substrate are determined to be retained bubbles;

[0042] (a2) Condition: The number of bubbles in a single plate of the obtained product glass substrate remains stable at x ± 3 per plate;

[0043] (b2) Condition: The number of bubbles in the single plate of the obtained product glass substrate remains stable at ≤0.5 / plate;

[0044] t0=0h; t1 is 1.5h-5h; t2 is at least 2h greater than t1; t3 is at least 2h greater than t2;

[0045] The ratio K of the number of bubbles with a diameter of 1-10 mm in any one of the obtained product glass substrates to the total number of bubbles in the product glass substrate is defined, and the number of bubbles in a single plate is x; in steps (3) and (4), K of the product glass substrate is ≥80%, and x is ≥2.

[0046] It should be noted that, in step (3), the moment of re-rotation is moment t2.

[0047] After being judged as trapped bubbles, although the number of bubbles in a single board can be maintained at a standard of ≤0.5 / board within a certain period of time, if it is not processed, the number of bubbles in a single board in the glass substrate will be ≥2 / board after 3-5 days, resulting in a decrease in the yield rate of the glass and seriously affecting the production efficiency.

[0048] The number of bubbles in the glass substrate described in the present invention is a statistical data of 10 glass substrates. For example, 0.3 / plate means that the total number of bubbles in the 10 glass substrates is 3, and not every glass substrate contains bubbles.

[0049] Preferably, the value of the number x of single-plate bubbles in the glass substrate is 2-10.

[0050] Preferably, the stirring speed of the stirring rod is 10-12 rpm.

[0051] The present invention has no particular limitation on the specific material and shape of the stirring rod. Those skilled in the art may select the stirring rod according to existing stirring rod products in the art. The present invention will not elaborate on this, and those skilled in the art should not understand it as a limitation on the present invention.

[0052] Preferably, in the condition (a1), the number of single-plate bubbles in the glass substrate first increases to 2-10 times x and then decreases.

[0053] Preferably, in the condition (b1), the number of single-plate bubbles in the glass substrate first increases to 2-10 times x and then decreases.

[0054] Preferably, each of the stable maintaining times is independently 2-3 hours.

[0055] The method for determining the source of bubbles in a glass substrate provided by the present invention requires that the glass liquid be kept flowing during the glass production process to continuously produce glass substrate products, the number of bubbles in the glass substrate products be continuously detected and monitored, and the source of the bubbles be determined based on the data obtained.

[0056] It should be noted that the determination method of the present invention is used to determine whether the bubble type in the glass substrate is clarified bubbles or retained bubbles, which does not mean that all bubbles contained in the glass substrate are clarified bubbles or retained bubbles, but means that clarified bubbles or retained bubbles are predominant, preferably more than 90% of the bubbles are clarified bubbles or retained bubbles. There may be other types of bubbles from other sources that are unavoidable on the glass production line, which will not be elaborated herein by the present invention, and those skilled in the art should not understand this as a limitation of the present invention.

[0057] The heating of the production line and equipment damage during normal production can cause trapped bubbles to form in the platinum channel mixing barrel. If the bubbles in the glass substrate are determined to be trapped bubbles, it is necessary to investigate the cause of the trapped bubbles and cut off the source of the trapped bubbles. The method for eliminating trapped bubbles provided by the present invention can reduce the trapped bubbles in the glass substrate and improve the yield rate of the glass.

[0058] As mentioned above, the second aspect of the present invention provides a method for eliminating trapped bubbles in a glass substrate, the method comprising:

[0059] S1: Keeping the glass liquid flowing continuously, lifting the stirring rod (2) in the platinum channel stirring barrel (1) into the retention layer (5) containing retained bubbles without penetrating the retention layer (5);

[0060] S2: starting the stirring rod (2) and stirring in the order of forward rotation, stop I, reverse rotation, and stop II as one stirring cycle; repeating the stirring cycle 0-5 times, so that the retained bubbles in the retention layer (5) enter the glass liquid in the stirring barrel (1);

[0061] S3: Stop rotating the stirring rod (2) to remove bubbles; the stirring rod (2) is stopped for more than 15 hours.

[0062] The "repeating stirring cycle 0-5 times" in the present invention means that only one stirring cycle is performed without repeating.

[0063] Preferably, in step S1, the diameter of the retained bubbles is ≤10 mm.

[0064] Preferably, the height of the stirring rod (2) entering the retaining layer (5) accounts for 50-80% of the total height of the retaining layer (5).

[0065] According to a preferred embodiment, in step S1, the diameter of the retained bubbles is 1-5 mm, and the height of the stirring rod (2) entering the retained layer (5) accounts for 50-60% of the total height of the retained layer (5).

[0066] According to another preferred embodiment, the diameter of the retained bubbles is 6-10 mm, and the height of the stirring rod (2) entering the retained layer (5) accounts for 65-80% of the total height of the retained layer (5).

[0067] In the present invention, after the stirring rod enters the retention layer, the height of the retention layer will be increased due to the volume of the stirring rod itself. The percentage of the height of the stirring rod entering the retention layer to the total height of the retention layer described in the present invention refers to the state after entering, rather than being calculated based on the height of the retention layer before entering.

[0068] Preferably, in step S2, the time of the forward rotation, the stop I, the reverse rotation and the stop II are each independently 10-20 minutes.

[0069] According to a preferred specific implementation, in step S2, the diameter of the retained bubbles in the retention layer (5) is 1-5 mm, and the time of the forward rotation, the stop I, the reverse rotation and the stop II are each independently 10-15 minutes.

[0070] According to another preferred specific implementation, in step S2, the diameter of the retained bubbles in the retention layer (5) is 6-10 mm, and the time of the forward rotation, the stop I, the reverse rotation and the stop II are each independently 16-20 minutes.

[0071] Preferably, in step S3, the stirring rod (2) is stopped for 15-30 hours.

[0072] Preferably, step S2 and step S3 are repeated 3-4 times. The inventors have found in their research that the treatment method under the preferred conditions can further reduce the number of trapped bubbles in the glass substrate and obtain a higher glass substrate yield.

[0073] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the raw materials used are all commercially available products.

[0074] Example 1

[0075] When the auxiliary heating device 4 on the upper part of the mixing barrel was abnormally shut down, the temperature of the upper space of the mixing barrel dropped rapidly by 100°C. The temperature of the mixing barrel 1 was automatically controlled, and the power compensation was 4kW. Automatic control means that the heaters in other parts of the mixing barrel increase the power through PID control to increase the overall temperature of the mixing barrel and increase the temperature of the upper part of the mixing barrel. After compensation, the temperature of the upper space of the mixing barrel dropped by 45°C. After a period of production, large bubble defects appeared on the glass plate surface, and the number of bubbles x of a single plate reached 5-10 / plate.

[0076] (1) After sampling and microscopic examination, the bubble sizes were concentrated in the range of 1-5 mm, which was similar to clarified bubbles. However, after the auxiliary heating device 4 on the upper part of the stirring barrel was abnormally shut down, the temperature of the stirring barrel space dropped by 45°C, which may have caused bubbles to be generated during the stirring process of the stirring rod 2 and retained in the retention layer 5 of the stirring barrel, and then flowed out after accumulating to a certain number.

[0077] (2) To quickly determine the source of the bubbles, stop stirring rod 2 (the speed before stopping is 12 rpm). After stopping for 1.5 h, the number of bubbles on the single plate increases to 82 / plate, and then gradually decreases. After 8 h, it decreases to 0.5 / plate and remains stable for 2 h. Start stirring rod 2, and the number of bubbles on the plate surface remains stable at 0.5 / plate for 2 h, which is determined to be trapped bubbles.

[0078] Moreover, the number of bubbles in the glass substrate increases to 3-5 per plate after 3d, because the stopped stirring rod 2 changes the flow trajectory of the glass liquid in the stirring barrel 1, brings out a part of the bubbles in the lower part of the retention layer 5, and gathers the bubbles that cannot be discharged to the wall of the stirring barrel 1. After the stirring rod 2 is started, the bubbles enter the stirring barrel 1 again with the glass liquid from the upper part of the retention layer 5. Due to the occurrence of this phenomenon, the accuracy of the judgment method provided by the present invention is further verified.

[0079] Comparative Example 1

[0080] During the production process, when large bubble defects appear on the glass plate surface, the number of bubbles x in a single plate reaches 5-10 / plate, and the bubble size is concentrated in the range of 1-5mm after sampling and microscopic examination, the traditional method of judging the source of glass bubbles is: based on experience, such bubbles are more likely to be clarified bubbles. The general countermeasures are to first increase the clarification temperature and change the kiln melting process. In order to prevent the clarification temperature from being too high, the clarification temperature is generally increased in steps by 2-3℃ each time, and observed for 1-2 days. According to the bubble situation, it is continued to increase. If there is no improvement in the bubbles by increasing 10-20℃, it will not be increased. If the kiln melting process is changed, it takes 7-10 days to see the effect of the adjustment. If the countermeasures of increasing the clarification temperature and changing the kiln melting process are effective, it is judged as clarified bubbles. If the countermeasures are ineffective, it is considered to be mixing tank 1 bubble, and then the countermeasures of mixing tank bubbles are switched.

[0081] Example 2

[0082] In Example 1, after it is determined that trapped bubbles are generated, the stirring barrel 1 is heated by 60° C. in order to cut off the source of bubble generation, increase the fluidity of the glass liquid in the trapped layer, and accelerate the discharge of trapped bubbles.

[0083] S1: In order to reduce trapped bubbles, the height of the stirring rod 2 is raised by 200 mm, and the stirring rod 2 enters the retention layer 5 of the stirring barrel (the height of the stirring rod entering the retention layer accounts for 50% of the total height of the retention layer);

[0084] S2: Start stirring rod 2, and perform stirring in the order of forward rotation for 15 minutes, stop for 15 minutes, reverse rotation for 15 minutes, and stop for 15 minutes as one stirring cycle; repeat the stirring cycle twice, the number of bubbles on the plate surface increases to 11.5 / plate, lower the height of stirring rod 2 to its original position, stop for 24 hours, the number of bubbles on the plate surface decreases to 0.2 / plate, and the number of bubbles on the plate surface stabilizes after starting stirring rod 2.

[0085] After three times of step S1 and step S2, the trapped bubbles were resolved, and the number of bubbles on the board surface was maintained below 0.3 per board. The yield rate reached 90%, and the production efficiency was guaranteed.

[0086] By comparing the methods of Example 1 and Comparative Example 1, it can be seen that the traditional judgment method needs to guess the source of bubbles based on experience and judge the source of bubbles based on the effect after the process countermeasures, which requires a lot of process adjustment and observation time. Misjudgment will extend the countermeasure cycle and bring some unnecessary process adjustments, weaken the stability of the production line, and may also cause some other glass defects such as platinum particles, needle-shaped platinum and other defects.

[0087] Therefore, the technical solution of the present invention is faster and more accurate. In addition, the method for eliminating trapped bubbles provided by the present invention is simple to operate, saves time, and has greater application value.

[0088] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for determining the type of bubbles in a glass substrate prepared by a continuous process, characterized in that: The method includes: (1) In a process of preparing a glass substrate by a continuous method, a glass liquid is introduced into a platinum channel stirring barrel with a stirring rod for stirring, and a material obtained after the stirring is subjected to a molding process to obtain a product glass substrate; (2) When the product glass substrate is a defective product, the stirring rod in the platinum channel stirring barrel is stopped and the timing is started as t0; (3) counting the number of bubbles in the single plate of the product glass substrate obtained from time t1 to time t2, and if it is found that the number of bubbles in the single plate of the product glass substrate meets condition (a1) or condition (b1) as time goes by, re-rotating the stirring rod in the platinum channel stirring barrel; (a1) Condition: The number of bubbles in a single plate of the obtained product glass substrate increases first and then decreases to x±3 / plate, and remains stable at x±3 / plate; (b1) Condition: The number of bubbles in a single plate of the obtained product glass substrate increases first and then decreases to ≤0.5 / plate, and remains stable at ≤0.5 / plate; (4) counting the number of bubbles in a single plate of the product glass substrate obtained from time t2 to time t3, and if it is found that as time passes, in the process that satisfies condition (a1) in step (3), the number of bubbles in a single plate of the product glass substrate meets condition (a2), then the bubbles in the product glass substrate are determined to be clear bubbles; if it is found that as time passes, in the process that satisfies condition (b1) in step (3), the number of bubbles in a single plate of the product glass substrate meets condition (b2), then the bubbles in the product glass substrate are determined to be retained bubbles; (a2) Condition: The number of bubbles in a single plate of the obtained product glass substrate remains stable at x ± 3 per plate; (b2) Condition: The number of bubbles in the single plate of the obtained product glass substrate remains stable at ≤0.5 / plate; t0=0h; t1 is 1.5h-5h; t2 is at least 2h greater than t1; t3 is at least 2h greater than t2; The ratio K of the number of bubbles with a diameter of 1-10 mm in any one of the obtained product glass substrates to the total number of bubbles in the product glass substrate is defined, and the number of bubbles in a single plate is x; in steps (3) and (4), K of the product glass substrate is ≥80%, and x is ≥2.

2. The method according to claim 1, characterized in that: The value of the number x of single-plate bubbles in the glass substrate is 2-20; and / or, The stirring speed of the stirring rod is 10-12 rpm.

3. The method according to claim 1 or 2, characterized in that: In the condition (a1), the number of single-plate bubbles in the glass substrate first increases to 2-10 times x and then decreases; And / or, in the condition (b1), the number of single-plate bubbles in the glass substrate first increases to 2-10 times x and then decreases.

4. The method according to any one of claims 1 to 3, characterized in that: Each of the stable maintaining time is independently 2-3 hours.

5. A method for eliminating trapped bubbles in a glass substrate, characterized in that: The method includes: S1: Keeping the glass liquid flowing continuously, lifting the stirring rod (2) in the platinum channel stirring barrel (1) into the retention layer (5) containing retained bubbles without penetrating the retention layer (5); S2: starting the stirring rod (2) and stirring in the order of forward rotation, stop I, reverse rotation, and stop II as one stirring cycle; repeating the stirring cycle 0-5 times, so that the retained bubbles in the retention layer (5) enter the glass liquid in the stirring barrel (1); S3: Stop rotating the stirring rod (2) to remove bubbles; the stirring rod (2) is stopped for more than 15 hours.

6. The method according to claim 5, characterized in that: In step S1, the diameter of the trapped bubbles is ≤10 mm; and / or, The height of the stirring rod (2) entering the retaining layer (5) accounts for 50-80% of the total height of the retaining layer (5).

7. The method according to claim 6, characterized in that: In step S1, the diameter of the retained bubbles is 1-5 mm, and the height of the stirring rod (2) entering the retention layer (5) accounts for 50-60% of the total height of the retention layer (5); and / or, The diameter of the retained bubbles is 6-10 mm, and the height of the stirring rod (2) entering the retained layer (5) accounts for 65-80% of the total height of the retained layer (5).

8. The method according to any one of claims 5 to 7, characterized in that: In step S2, the time of the forward rotation, the stop I, the reverse rotation and the stop II are each independently 10-20 minutes.

9. The method according to claim 8, characterized in that In step S2, the diameter of the retained bubbles in the retention layer (5) is 1-5 mm, and the time of the forward rotation, the stop I, the reverse rotation and the stop II are each independently 10-15 min; and / or, In step S2, the diameter of the retained bubbles in the retention layer (5) is 6-10 mm, and the time of the forward rotation, the stop I, the reverse rotation and the stop II are each independently 16-20 minutes.

10. The method according to any one of claims 5 to 9, characterized in that: In step S3, the stirring rod (2) is stopped for 15-30 hours.

Citation Information

Patent Citations

  • Method for improving membrane flux by using micro-stirring

    CN113546519A

  • Method for eliminating bubbles in molten glass, application of method, molten glass and application of molten glass

    CN113830995A

  • High-efficiency clarification platinum channel adopting graded bubble removal

    CN115093106A

  • Method for removing bubbles in glass substrate production

    CN118307177A