Optical glass and optical element
By adjusting the proportions of SiO2, B2O3, and ZrO2/Nb2O5, the existing optical glass quality deterioration and volatilization problems are solved, high-quality optical glass and optical elements with refractive index and Abbe number within the required range are achieved, and color reduction is achieved. Aberration.
Patent Information
- Application Number
- CN202410252590.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-06
- Publication Date
- 2024-10-01
AI Technical Summary
Existing optical glass has limitations in refractive index and Abbe number, and contains a large amount of B2O3 components, resulting in poor quality and volatilization problems. It is difficult to obtain high quality with a refractive index below 1.64000, an Abbe number below 43.00, and a small partial dispersion ratio. Optical glass.
By adjusting the proportions of SiO2, B2O3, and ZrO2/Nb2O5 to a range of 0.200 to 0.900, we can rationally prepare optical glass with a refractive index and Abbe number within the required range, ensuring a small partial dispersion ratio and high quality.
It has achieved high-quality optical glass and optical elements with a refractive index of less than 1.64000, an Abbe number of less than 43.00, and a small partial dispersion ratio, reducing glass quality deterioration and texture generation, and improving the performance of the optical system.
Smart Images

Figure CN118724461A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to optical glass and optical element. Background Art
[0002] Optical glass and optical elements can be used to improve the optical characteristics of cameras and imaging devices by combining lenses with different optical regions, or can be installed in optical devices to realize various optical designs.
[0003] Optical systems, regardless of their size, all contain aberrations called "color bleeding." These aberrations are classified into monochromatic aberrations and chromatic aberrations, and chromatic aberrations, in particular, strongly depend on the material properties of the lenses used in the optical system.
[0004] Chromatic aberration can be offset by combining a high-dispersion lens and a low-dispersion lens, or a lens with a relatively large partial dispersion and a lens with a relatively small partial dispersion. However, it is difficult to obtain optical glass with low dispersion and a small partial dispersion ratio due to material properties.
[0005] In addition, in order to promote the stability of the glass, the optical glass containing the Nb2O5 component contains a specified amount of SiO2 component and B2O3 component.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2008-297198
[0009] Patent Document 2: Japanese Patent Application Publication No. 2016-222511 Summary of the invention
[0010] Technical problem to be solved by the invention
[0011] The optical glass disclosed in Patent Document 1 does not describe the refractive index (n d ) is less than 1.64000, and the Abbe number (ν d ) is glass below 43.00.
[0012] The optical glass disclosed in Patent Document 2 describes the refractive index (n d ) is less than 1.64000, and the Abbe number (ν d ) is a glass below 43.00, but contains a large amount of B2O3 components.
[0013] Glass containing a large amount of B2O3 components has a higher possibility of texture generation due to volatilization of the B2O3 components and quality deterioration accompanying the volatilization.
[0014] The present invention is proposed based on the above technical problems, and its purpose is to obtain a refractive index (n d ) is less than 1.64000, and the Abbe number (ν d ) is less than 43.00, and the partial dispersion ratio is small and the quality is high.
[0015] Solutions to technical problems
[0016] The inventors of the present invention have conducted repeated experiments and studies to solve the above-mentioned technical problems, and have found that by containing SiO2 and B2O3 components and making the mass ratio of ZrO2 / Nb2O5 within the range of 0.200 to 0.900, it is possible to obtain an optical glass having a refractive index and an Abbe number within the required range, a small partial dispersion ratio and high quality, thereby completing the present invention.
[0017] Specifically, the present invention provides the following products.
[0018] (1) An optical glass, wherein:
[0019] Refractive index (n d ) is below 1.64000,
[0020] Abbe number (ν d ) is below 43.00,
[0021] Measured in mass % based on oxides,
[0022] SiO2 content is 20.00~50.00%,
[0023] B2O3 content is greater than 0% and less than or equal to 25.0%,
[0024] The mass ratio ZrO2 / Nb2O5 is 0.200~0.900.
[0025] (2) An optical element made of the optical glass described in (1).
[0026] Effects of the Invention
[0027] According to the present invention, a refractive index (n d ) is less than 1.64000, and the Abbe number (ν d ) is less than 43.00, and the partial dispersion ratio is small and the quality of optical glass and optical elements is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The partial dispersion ratio (θg, F) and the Abbe number (ν d )’s relationship diagram. DETAILED DESCRIPTION
[0029] Hereinafter, the embodiments of the optical glass of the present invention will be described in detail. The present invention is not limited to the following embodiments, and can be appropriately changed and implemented within the scope of the purpose of the present invention. It should be noted that the description of the repeated parts may be appropriately omitted, which will not limit the purpose of the invention.
[0030] [Glass composition]
[0031] The composition range of each component constituting the optical glass of the present invention is as follows. In this specification, unless otherwise specifically denied, the content of each component is expressed in mass % relative to the total mass of the glass in oxide conversion composition. Here, "oxide conversion composition" means that, assuming that the oxides, complex salts, metal fluorides, etc. used as raw materials of the glass composition components of the present invention are all decomposed and converted into oxides during melting, the total mass of the generated oxides is recorded as 100 mass %, and the composition of each component contained in the glass is expressed.
[0032] SiO2 is a component that promotes the formation of stable glass.
[0033] In particular, by making the content of SiO2 component 20.0% or more, not only the partial dispersion ratio is greatly improved, but also devitrification can be reduced and moldability can be improved. Therefore, the lower limit of the content of SiO2 component is preferably 20.0% or more, more preferably 23.00% or more, more preferably 25.0% or more, further preferably 27.0% or more, further preferably 30.0% or more, further preferably 32.0% or more, and further preferably 35.0% or more.
[0034] On the other hand, by making the content of SiO2 component 50.0% or less, the increase of partial dispersion ratio can be suppressed. In addition, the reduction of solubility of glass raw material can be suppressed thereby. Therefore, the content of SiO2 component has an upper limit preferably of 50.0% or less, more preferably of 48.0% or less, still more preferably of 47.0% or less, further preferably of 46.0% or less, and still more preferably of 45.0% or less.
[0035] The B2O3 component can promote stable glass formation and reduce devitrification, and can improve the solubility of glass raw materials. Therefore, the lower limit of the content of the B2O3 component is preferably greater than 0%, more preferably 1.0% or more, even more preferably 3.0% or more, further preferably 5.0% or more, further preferably 8.0% or more, and further preferably 10.0% or more.
[0036] On the other hand, by making the content of B2O3 component less than 25.0%, the deterioration of glass quality and the increase of partial dispersion ratio can be suppressed. B2O3 component is a component that is easily volatile. By suppressing volatilization, the generation of texture and the deterioration of glass quality can be suppressed. The upper limit of the content of B2O3 component is preferably less than 25.0%, more preferably less than 23.0%, more preferably less than 20.0%, further preferably less than 18.0%, further preferably less than 15.0%, further preferably less than 13.0%, and further preferably less than 11.0%.
[0037] The Nb2O5 component is a component that can reduce the Abbe number and the partial dispersion ratio. Therefore, the lower limit of the content of the Nb2O5 component is preferably 5.0% or more, more preferably 8.0% or more, even more preferably 10.0% or more, further preferably 12.0% or more, and even more preferably 15.0% or more.
[0038] On the other hand, the refractive index can be reduced by making the content of Nb2O5 component 40.0% or less. Therefore, the upper limit of the content of Nb2O5 component is preferably 40.0% or less, more preferably 35.0% or less, still more preferably 30.0% or less, further preferably 28.0% or less, and further preferably 25.0% or less.
[0039] By making the content of Li2O component 10.0% or less, the increase of refractive index can be suppressed, the deterioration of reheating compressibility can be reduced, and the devitrification caused by excessive content can be reduced. Therefore, the upper limit of the content of Li2O component is preferably 10.0% or less, more preferably 7.0% or less, more preferably 5.0% or less, more preferably 4.0% or less, further preferably 3.0% or less, further preferably 2.0% or less, and further preferably 1.0% or less.
[0040] By making the content of K2O component 10.0% or less, the deterioration of reheating compressibility can be reduced, and the devitrification caused by excessive content can be reduced. Therefore, the upper limit of the content of K2O component is preferably 10.0% or less, more preferably 7.0% or less, still more preferably 5.0% or less, and further preferably 3.0% or less.
[0041] The Na2O component can reduce the partial dispersion ratio of the glass and improve the solubility of the glass raw material. Therefore, the lower limit of the content of the Na2O component is preferably 3.0% or more, more preferably 4.0% or more, even more preferably 5.0% or more, further preferably 7.0% or more, further preferably 10.0% or more, further preferably 11.0% or more, and further preferably 12.0% or more.
[0042] On the other hand, by making the content of Na2O component 25.0% or less, devitrification caused by excessive content can be reduced. Therefore, the upper limit of the content of Na2O component is preferably 25.0% or less, more preferably 23.0% or less, still more preferably 20.0% or less, and further preferably 18.0% or less.
[0043] By making the content of the MgO component 10.0% or less, the increase in the refractive index can be suppressed and devitrification can be reduced. Therefore, the upper limit of the content of the MgO component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and further preferably 1.0% or less.
[0044] By making the content of the CaO component 10.0% or less, the increase in the refractive index can be suppressed and devitrification can be reduced. Therefore, the upper limit of the content of the CaO component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and further preferably 1.0% or less.
[0045] By making the content of BaO component 10.0% or less, the increase of refractive index and Abbe number can be suppressed, and devitrification can be reduced. Therefore, the upper limit of the content of BaO component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and further preferably 1.0% or less.
[0046] By making the content of the SrO component 10.0% or less, the decrease in the refractive index and the increase in the Abbe number can be suppressed, and devitrification can be reduced. Therefore, the upper limit of the content of the SrO component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and further preferably 1.0% or less.
[0047] The ZrO2 component can increase the refractive index of the glass, reduce the Abbe number, reduce the partial dispersion ratio, and reduce devitrification. In addition, devitrification and coloration during reheating can be reduced. Therefore, the lower limit of the content of the ZrO2 component is preferably greater than 0%, more preferably 1.0% or more, even more preferably 2.0% or more, further preferably 3.0% or more, and even more preferably 4.0% or more.
[0048] On the other hand, by making the content of ZrO2 component less than 25.0%, devitrification caused by excessive content can be reduced, and more homogeneous glass can be easily obtained. Therefore, the content of ZrO2 component has an upper limit preferably of less than 25.0%, more preferably less than 20.0%, still more preferably less than 15.0%, and further preferably less than 13.0%.
[0049] By making the content of TiO2 component 10.0% or less, the increase of refractive index and dispersion caused by excessive content can be suppressed. Therefore, the upper limit of the content of TiO2 component is preferably 10.0% or less, more preferably 8.0% or less, still more preferably 7.0% or less, still more preferably 5.0% or less, further preferably 3.0% or less, still more preferably 2.0% or less, and still more preferably 1.0% or less.
[0050] Although WO3 and Bi2O3 increase the refractive index of glass, their high content may cause coloration of the glass and increase the specific gravity. The preferred ranges of WO3 and Bi2O3 are as follows.
[0051] The upper limit of the content of the WO3 component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, further preferably 1.0% or less, and the content may be 0%.
[0052] The upper limit of the content of the Bi2O3 component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, further preferably 1.0% or less, and the content may also be 0%.
[0053] When the content of La2O3, Y2O3, Gd2O3 and Yb2O3 is high, the refractive index increases, the stability is impaired and the specific gravity increases. The preferred ranges of La2O3, Y2O3, Gd2O3 and Yb2O3 are as follows.
[0054] The upper limit of the La2O3 content is preferably below 12.0%, more preferably less than 10.0%, even more preferably below 8.0%, further preferably below 5.0%, further preferably below 3.0%, and even more preferably below 1.0%. The content may also be 0%.
[0055] The upper limit of the content of the Y2O3 component is preferably 10.0% or less, more preferably 8.0% or less, still more preferably 5.0% or less, further preferably 3.0% or less, and most preferably 1.0% or less. The content may also be 0%.
[0056] The upper limit of the content of Gd2O3 component is preferably less than 8.0%, more preferably below 5.0%, even more preferably below 3.0%, further preferably below 2.0%, further preferably below 1.0%, and most preferably below 0.5%. The content can also be 0%.
[0057] The upper limit of the content of the Yb2O3 component is preferably 8.0% or less, more preferably 5.0% or less, still more preferably 2.0% or less, further preferably 1.0% or less, and most preferably 0.5% or less. The content may also be 0%.
[0058] The Al2O3 component can reduce the refractive index and dispersion. Therefore, the content of the Al2O3 component is preferably greater than 0%, more preferably greater than 0.5%, even more preferably greater than 1.0%, and further preferably 1.5%. In particular, by making the content of the Al2O3 component 10.0% or less, the meltability of the glass can be improved and the devitrification tendency of the glass can be reduced. Therefore, the content of the Al2O3 component is preferably less than 10.0%, more preferably less than 8.0%, and even more preferably less than 6.0%.
[0059] The ZnO component is a component that improves the resistance of glass to devitrification. In particular, by making the content of the ZnO component 5.0% or less, the specific gravity can be reduced and a glass with a low refractive index can be easily obtained. Therefore, the upper limit of the content of the ZnO component is preferably 5.0% or less, more preferably 3.0% or less, and most preferably 1.0% or less, and the content may also be 0%.
[0060] Ta2O5 is a component that improves the resistance of glass to devitrification. On the other hand, by making the content of Ta2O5 component less than 5.0%, the usage of Ta2O5 component as a rare mineral resource can be reduced, and the glass is easy to melt at a lower temperature, so the production cost of the glass can be reduced. In addition, thereby, the devitrification of the glass caused by excessive inclusion of Ta2O5 component can be reduced and the specific gravity can be reduced. Therefore, the content of Ta2O5 component has an upper limit preferably of less than 5.0%, more preferably less than 3.0%, and even more preferably less than 1.0%, and the content can also be 0%.
[0061] The upper limit of the content of the P2O5 component is preferably 5.0% or less, more preferably 3.0% or less, still more preferably 1.0% or less, further preferably 0.5% or less, and the content may be 0%.
[0062] The upper limit of the content of the component F is preferably 5.0% or less, more preferably 3.0% or less, still more preferably 1.0% or less, further preferably 0.5% or less, further preferably 0.3% or less, and the content may be 0%.
[0063] The upper limit of the content of TeO2 component is preferably 3.0% or less, more preferably 2.0% or less, still more preferably 1.0% or less, further preferably 0.5% or less, and the content may also be 0%.
[0064] The upper limit of the content of the GeO2 component is preferably 3.0% or less, more preferably 2.0% or less, still more preferably 1.0% or less, further preferably 0.5% or less, and the content may also be 0%.
[0065] The upper limit of the content of the CeO2 component is preferably 3.0% or less, more preferably 2.0% or less, still more preferably 1.0% or less, further preferably 0.5% or less, and the content may be 0%.
[0066] The content of the Er2O3 component and the Pr2O3 component is preferably 1.0% or less, more preferably 0.5% or less, still more preferably 0.1% or less, and most preferably substantially free of them.
[0067] The upper limit of the content of the SnO2 component is preferably 2.0% or less, more preferably 1.0% or less, further preferably 0.5% or less, and the content may be 0%.
[0068] The Sb2O3 component is an arbitrary component that promotes clarification and defoaming when melting glass. Among them, by making the content of the Sb2O3 component less than 0.20%, it is particularly possible to suppress coloring in high-refractive index glass. In addition, by making it less than 0.20%, it is difficult to produce excessive foaming when the glass is melted, so it is possible to make the Sb2O3 component difficult to alloy with melting equipment (especially precious metals such as Pt). Therefore, the content of the Sb2O3 component is preferably less than 0.20%, more preferably less than 0.10%, and further preferably less than 0.08%, and the content can also be 0%.
[0069] It should be noted that the component that clarifies and defoams the glass is not limited to the above-mentioned Sb2O3 component, and clarifiers, defoamers or combinations thereof known in the field of glass manufacturing can be used.
[0070] The C component can maintain the reducing atmosphere in the platinum crucible, suppress the mixing of platinum into the glass due to oxidation, and improve the transmittance. However, if the content is too high, the cationic components in the glass will be reduced, and the glass will be colored. Therefore, the upper limit of the content of the C component is preferably 10.0% or less, more preferably 8.0% or less, even more preferably 6.0% or less, and most preferably 5.0% or less. On the other hand, the lower limit of the content of the C component is preferably greater than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and most preferably 2.0% or more. The content may also be 0%.
[0071] The S component can maintain the reducing atmosphere in the platinum crucible, suppress the mixing of platinum into the glass due to oxidation, and improve the transmittance. However, if the content is too high, the cationic components in the glass will be reduced, and the glass will be colored. Therefore, the upper limit of the content of the S component is preferably 10.0% or less, more preferably 8.0% or less, even more preferably 6.0% or less, and most preferably 5.0% or less. On the other hand, the lower limit of the content of the S component is preferably greater than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and most preferably 2.0% or more. The content may also be 0%.
[0072] Organic components such as sucrose can maintain the reducing atmosphere in the platinum crucible, inhibit the mixing of platinum into the glass due to oxidation, and improve the transmittance. However, if the content is too high, the cationic components in the glass will be reduced, and the glass will be colored. Therefore, the upper limit of the content of organic components such as sucrose is preferably 10.0% or less, more preferably 8.0% or less, even more preferably 6.0% or less, and most preferably 5.0% or less. On the other hand, the lower limit of the content of organic components such as sucrose is preferably greater than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and most preferably 2.0% or more. The content may also be 0%.
[0073] By making the sum (mass sum) of the contents of the Ln2O3 component (wherein Ln is one or more selected from the group consisting of La, Y, Gd, and Yb) 12.0% or less, it is possible to suppress devitrification caused by excessive content and maintain the refractive index. Therefore, the upper limit is preferably 12.0% or less, more preferably less than 10.0%, still more preferably 8.0% or less, further preferably 6.0% or less, further preferably 4.0% or less, and further preferably 2.0% or less, and the content may also be 0%.
[0074] By making the sum of the contents of Rn2O components (wherein Rn is one or more selected from the group consisting of Li, Na, and K) less than 5.0%, the solubility of the glass raw material can be improved, the low transformation point can be maintained, and the partial dispersion ratio can be reduced. Therefore, the lower limit of the sum of the contents of Rn2O components is preferably 5.0% or more, more preferably 8.0% or more, even more preferably 10.0% or more, further preferably 12.0% or more, and further preferably 13.0% or more. On the other hand, by making the sum of the contents of Rn2O components less than 25.0%, the increase in the Abbe number can be suppressed. The upper limit of the sum of the contents of Rn2O components is preferably 25.0% or less, more preferably 23.0% or less, even more preferably 20.0% or less, and further preferably 18.0% or less.
[0075] By making the sum of the contents of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, and Ba) 10.0% or less, the increase in the Abbe number can be suppressed, and the devitrification of the glass caused by the excessive contents of these components can be reduced. Therefore, the upper limit of the mass sum of the RO components is preferably 25.0% or less, more preferably less than 15.0%, even more preferably less than 10.0%, further preferably less than 5.0%, and further preferably less than 2.0%.
[0076] By making the ratio of ZrO2 to the Nb2O5 component, that is, the mass ratio ZrO2 / Nb2O5, 0.900 or less, the resistance to devitrification can be improved. The upper limit of the mass ratio ZrO2 / Nb2O5 is preferably 0.900 or less, more preferably 0.870 or less, even more preferably 0.850 or less, even more preferably 0.830 or less, further preferably 0.800 or less, even more preferably 0.780 or less, and even more preferably 0.750 or less. On the other hand, by making the mass ratio ZrO2 / Nb2O5 0.200 or more, the partial dispersion ratio can be reduced, and the Abbe number can be reduced. Therefore, the lower limit of the mass ratio Nb2O5 / ZrO2 is preferably 0.200 or more, more preferably 0.230 or more, and even more preferably 0.250 or more.
[0077] When the total content of SiO2 and B2O3, i.e., the mass sum SiO2+B2O3, is 27.0% or more, the devitrification resistance and chemical durability of the glass can be improved. The mass sum SiO2+B2O3, its lower limit is preferably 27.0% or more, more preferably 30.0% or more, even more preferably 33.0% or more, and further preferably 35.0% or more. On the other hand, when the mass sum SiO2+B2O3 is 50.0% or less, the stability degradation caused by the excess content can be suppressed. Therefore, the mass sum SiO2+B2O3, its upper limit is preferably 50.0% or less, more preferably 53.0% or less, even more preferably 50.0% or less, and further preferably 48.0% or less.
[0078] When the total content of Nb2O5 and ZrO2, i.e., the mass sum of Nb2O5+ZrO2, is 20.0% or more, it is possible to reduce the partial dispersion ratio, achieve high dispersion, and improve chemical durability. The lower limit of the mass sum of Nb2O5+ZrO2 is preferably 20.0% or more, more preferably 23.0% or more, even more preferably 25.0% or more, and further preferably 27.0% or more. On the other hand, when the mass sum of Nb2O5+ZrO2 is 40.0% or less, the deterioration of stability caused by excessive content can be suppressed. Therefore, the upper limit of the mass sum of Nb2O5+ZrO2 is preferably 40.0% or less, more preferably 38.0% or less, even more preferably 35.0% or less, and further preferably 33.0% or less.
[0079] By making the sum of the contents of SiO2 and B2O3 components compared to the sum of the contents of Rn2O components, that is, the mass ratio (SiO2+B2O3) / Rn2O, greater than 0 and less than 10.0, the devitrification resistance and chemical durability of the glass can be improved, the reheating press moldability can be good, and the reduction of the refractive index can be suppressed. The lower limit of the mass ratio (SiO2+B2O3) / Rn2O is preferably greater than 0, more preferably greater than 1.00, more preferably greater than 2.00, and further preferably greater than 3.00. On the other hand, the upper limit of the mass ratio (SiO2+B2O3) / Rn2O is preferably less than 10.0, more preferably less than 8.00, still more preferably less than 7.00, and further preferably less than 6.00.
[0080] <About ingredients that should not be contained>
[0081] Next, components that should not be contained in the optical glass of the present invention and components that are preferably not contained are described.
[0082] Other components can be added as needed within the range that does not impair the characteristics of the glass of the present invention. However, in addition to Ti, Zr, Nb, W, La, Gd, Y, Yb, and Lu, various transition metal components such as Nd, V, Cr, Mn, Fe, Co, Ni, Cu, Ag, and Mo have the property of coloring the glass even in a small amount when contained alone or in a composite form, and absorbing light of a specific wavelength in the visible light region. Therefore, it is preferably substantially not contained in optical glasses using wavelengths in the visible light region.
[0083] In addition, since lead compounds such as PbO and arsenic compounds such as As2O3 are components with high environmental burden, it is preferable that they are substantially not contained, that is, they are not contained at all except for unavoidable contamination.
[0084] In addition, Th, Cd, Tl, Os, Be and Se are each considered harmful chemical substances and are therefore avoided in recent years. Environmental measures must be taken not only in the glass manufacturing process but also in the processing process and until the waste treatment after the glass is manufactured. Therefore, when the environmental impact is important, it is preferred that these components are not substantially contained.
[0085] [physical properties]
[0086] The refractive index (n d ), and its upper limit is preferably 1.64000 or less, more preferably 1.63500 or less, and still more preferably 1.63000 or less. On the other hand, the refractive index (n d ), the lower limit of which is preferably 1.58000 or more, more preferably 1.59000 or more, and still more preferably 1.60000 or more. On the other hand, the Abbe number (ν d )The Abbe number (ν d ), the upper limit of which is preferably 43.00 or less, more preferably 42.50 or less, and still more preferably 42.00 or less. On the other hand, the Abbe number (ν d ), the lower limit of which is preferably 35.00 or more, more preferably 36.00 or more, still more preferably 38.00 or more.
[0087] The optical glass of the present invention has a relatively low partial dispersion ratio (θg, F).
[0088] More specifically, the upper limit of the partial dispersion ratio (θg, F) of the optical glass of the present invention is preferably 0.586 or less, more preferably 0.585 or less, and still more preferably 0.584 or less.
[0089] As a result, an optical glass having a low partial dispersion ratio (θg, F) can be obtained, and an optical element formed of the optical glass can play a role in reducing chromatic aberration of an optical system.
[0090] On the other hand, the optical glass of the present invention has a partial dispersion ratio (θg, F) and an Abbe number (ν d ), preferably satisfying θg, F≤(-0.00187×ν d +0.651), it is more preferable to satisfy θg, F≤(-0.00187×ν d +0.650), and more preferably, θg, F≤(-0.00187×ν d +0.649), and more preferably, θg, F≤(-0.00187×ν d +0.648).
[0091] Furthermore, the optical glass of the present invention has a small anomalous dispersion (Δθg, F), and therefore a lens capable of correcting chromatic aberration with high accuracy can be easily obtained.
[0092] The upper limit of the anomalous dispersion (Δθg, F) is preferably -0.0020 or less, more preferably -0.0030 or less, still more preferably -0.0040 or less, and further preferably -0.0050 or less.
[0093] Generally, chromatic aberration can be corrected by combining a low-dispersion convex lens and a high-dispersion concave lens, but this combination can only correct the aberrations in the red and green regions, and the aberrations in the blue region still remain. The aberrations in the blue region that are not completely removed are called secondary spectrum. In order to correct the secondary spectrum, it is necessary to consider the trend of the g-line (435.835nm) in the blue region for optical design. At this time, the partial dispersion ratio (θg, F) is used as an indicator of optical characteristics that are of concern in optical design. In the above-mentioned optical system in which a low-dispersion lens and a high-dispersion lens are combined, the secondary spectrum can be well corrected by using an optical material with a larger partial dispersion ratio (θg, F) for the lens on the low-dispersion side and an optical material with a smaller partial dispersion ratio (θg, F) for the lens on the high-dispersion side.
[0094] The partial dispersion ratio (θg, F) is expressed by the following equation (1).
[0095] θg, F=(ng-n F ) / (n F -n C )······(1)
[0096] In optical glass, the partial dispersion ratio (θg, F) and the Abbe number (ν d ) has a nearly linear relationship. The straight line representing this relationship is a line with the vertical axis representing the partial dispersion ratio (θg, F) and the horizontal axis representing the Abbe number (ν d ) on the orthogonal coordinates of NSL7 and PBM2, and the partial dispersion ratio and Abbe number of NSL7 and PBM2 are plotted, and the straight line connecting the two points is represented and called the standard line. The standard glass used as the basis of the standard line varies according to each optical glass manufacturer, but each company uses roughly the same slope and intercept to define it. (NSL7 and PBM2 are optical glasses manufactured by Obara Co., Ltd., and the Abbe number of PBM2 (ν d ) is 36.3, the partial dispersion ratio (θg, F) is 0.5828, and the Abbe number (ν d ) is 60.5, and the partial dispersion ratio (θg, F) is 0.5436. )
[0097] [Manufacturing method]
[0098] The optical glass of the present invention can be produced, for example, as follows. That is, the above raw materials are uniformly mixed so that each component is within a specified content range, and the prepared mixture is placed in a platinum crucible. Depending on the melting difficulty of the glass raw materials, an electric furnace is used to melt them at a temperature range of 1100° C. to 1400° C. for 1.5 to 5 hours, and after stirring to homogenize them, the temperature is lowered to an appropriate level, and then cast in a mold and slowly cooled to produce the glass. The melting can be carried out in a quartz crucible and then in a platinum crucible.
[0099] [Glass molding]
[0100] The glass of the present invention can be melted and molded by a known method. It should be noted that the method for molding the glass melt is not limited.
[0101] [Optical components]
[0102] The glass molded body can be produced from the produced optical glass by a grinding method, or a compression molding method such as reheating compression molding, precision compression molding, etc. That is, the optical glass can be subjected to mechanical processing such as cutting and grinding to produce the glass molded body. In addition, the method for producing the glass molded body is not limited to the above methods.
[0103] Thus, the optical glass of the present invention can be used in a variety of optical elements and optical designs. Among them, optical elements such as lenses and prisms are particularly preferred. Thus, the optical element can be made lightweight, and when used in optical equipment such as cameras and projectors, high-precision and high-definition imaging characteristics and projection characteristics can be achieved.
[0104] [Example]
[0105] The compositions of the embodiments and comparative examples of the glasses of the present invention, and the refractive index (n d ), Abbe number (ν d ), partial dispersion ratio (θg, F), and anomalous dispersion (Δθg, F) are shown in Tables 1 to 4. The glass of the comparative example is the glass of Example 1 of Japanese Patent Application Laid-Open No. 2008-297198.
[0106] The glass of the embodiments of the present invention uses high-purity raw materials such as oxides, hydroxides, carbonates, nitrates, thiochlorides, fluorides, metaphosphate compounds, etc., which are commonly used for optical glass, as raw materials for each component. These raw materials are weighed and uniformly mixed in the proportions of the compositions of the embodiments shown in the table, and then put into a platinum crucible. Depending on the melting difficulty of the glass raw materials, they are melted in an electric furnace at a temperature range of 1100 to 1400° C. for 1.5 to 5 hours, stirred to homogenize, cast in a mold, and slowly cooled to produce glass.
[0107] The refractive index of the glass of the embodiment (n d ), Abbe number (ν d ), partial dispersion ratio (θg, F), and anomalous dispersion (Δθg, F) are measured in accordance with the V-block method specified in JIS B 7071-2: 2018. Here, the refractive index (n d ), expressed as the measured value of the d line (587.56nm) of a helium lamp. In addition, the Abbe number (ν d ), using the refractive index for the d-line of a helium lamp (n d ), the refractive index (n F ), the refractive index (n C ) value, according to the Abbe number (ν d )=[(n d -1) / (n F -n C )] can be calculated. These refractive indices (n d ), Abbe number (ν d ) is obtained by measuring a glass obtained by slowly cooling the temperature at a rate of -25°C / hr.
[0108] And, according to the obtained Abbe number (ν d ) and the partial dispersion ratio (θg, F), and find the relationship (θg, F = -a × ν d +b) is the intercept b when the slope a is 0.00187.
[0109] Then, a straight line connecting two points representing the partial dispersion ratio and Abbe number of NSL7 and PBM2 is drawn based on the standard line (. NSL7 and PBM2 are optical glasses manufactured by Ohara Co., Ltd., and the Abbe number of PBM2 (ν d ) is 36.3, the partial dispersion ratio (θg, F) is 0.5828, and the Abbe number (ν d) is 60.5, and the partial dispersion ratio (θg, F) is 0.5436. The anomalous dispersion (Δθg, F) is calculated by taking the difference between the value of the partial dispersion ratio (θg, F) on ) and the value of the measured partial dispersion ratio (θg, F).
[0110]
Table 1
[0111]
[0112]
Table 2
[0113]
[0114]
Table 3
[0115]
[0116]
Table 4
[0117]
[0118] As shown in the table, the glass of the embodiments of the present invention has a refractive index (n d ) are all below 1.64000, and the Abbe number (ν d ) are all below 43.00, within the required range.
[0119] It can be seen that the optical glass of the embodiment has an Abbe number (ν d ) is within the required range and the partial dispersion ratio (θg, F) is small.
[0120] Although the present invention has been described in detail above for the purpose of illustration, the purpose of the present embodiment is only for illustration, and it should be fully understood that those skilled in the art can make many changes to the present invention without departing from the spirit and scope of the present invention.
Claims
1. An optical glass, wherein: Refractive index (n d ) is below 1.64000, Abbe number (ν d ) is below 43.00, Calculated as mass % based on oxide: SiO2 content is 20.00~50.00%, B2O3 content is greater than 0% and less than or equal to 25.0%, The mass ratio ZrO2 / Nb2O5 is 0.200~0.
900.