Salt as well as preparation method and application thereof
By using an inner salt type monofluoro-substituted alkenyl sulfonate as a photoacid generator, combined with an acid deprotection resin and a solvent, a chemically amplified resist composition is formed, which solves the problem of exposure energy margin of traditional photoacid generators. Solve the problem of deficiencies and achieve high-precision patterning and high-quality component preparation.
Patent Information
- Application Number
- CN202410788882.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
AI Technical Summary
While traditional photoacid generators improve resolution and pattern roughness, their exposure energy margin is poor, making it difficult to meet the needs of high-precision patterning.
Provide a monofluorine-substituted alkenyl sulfonate with an inner salt structure, used as a photoacid generator to reduce the diffusion coefficient of the acid, increase the exposure energy margin, and combine with the acid deprotection resin and solvent to form Chemically amplified resist composition.
It improves the exposure energy margin, enhances the exposure performance of the resist layer, is suitable for semiconductor patterning processes, obtains high-quality small-size patterns, and improves the preparation precision and efficiency of components.
Smart Images

Figure CN118724775A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of compounds, and in particular to a salt and a preparation method and application thereof. Background Art
[0002] Chemically amplified photoresists mainly include polymer resins and photoacid generators (PAGs). The photoacid generator generates acid when irradiated by active light or radiation, and the main chain or branched chain of the polymer resin in the exposed or irradiated part reacts with the generated acid and is decomposed or cross-linked in a so-called "post-exposure baking" (PEB) manner, so that the polarity of the polymer resin is changed. This change in polarity causes a solubility difference in the developing solution between the irradiated exposed area and the unexposed area, thereby forming a positive or negative image of the mask on the substrate. Each photochemically generated catalyst molecule can promote many solubility conversion reaction events, and the initial exposure dose is "amplified" by a subsequent series of chemical reaction events.
[0003] Energy Latitude (EL) refers to the maximum allowable deviation of exposure energy within the allowable range of line width variation. While traditional photoacid generators can improve resolution and pattern roughness, their exposure energy latitude (EL) is generally poor, and there is room for improvement. Summary of the invention
[0004] The present application provides a salt and a preparation method and application thereof to improve the exposure energy margin.
[0005] The present application also provides a chemically amplified resist composition comprising the above salt and application thereof.
[0006] The first aspect of the present application provides a salt having a structure shown in Formula 1:
[0007]
[0008] In Formula 1, M1 is selected from a substituted or unsubstituted first cyclic group, the first cyclic group includes N1 substituted or unsubstituted cyclic groups, N1≥1, when N1=1, the cyclic group is a benzene ring, when N1>1, at least one cyclic group among the N1 cyclic groups is a benzene ring; M2 is selected from a substituted or unsubstituted second cyclic group, the second cyclic group includes N2 substituted or unsubstituted cyclic groups, N2≥1, when N2=1, the cyclic group is a benzene ring, when N2>1, at least one cyclic group among the N2 cyclic groups is a benzene ring; M3 is selected from a substituted or unsubstituted third cyclic group, the third cyclic group includes N3 substituted or unsubstituted cyclic groups, N3≥1, when N3=1, the cyclic group is a benzene ring, when N3>1, at least one cyclic group among the N3 cyclic groups is a benzene ring;
[0009] Q1, Q2, Q3 are independently a single bond, a heteroatom, a divalent hydrocarbon group with 1-20 carbon atoms which may or may not contain heteroatoms, or do not exist; X is a divalent connecting group; L1 is selected from a single bond, a divalent hydrocarbon group with 1-20 carbon atoms which may or may not contain heteroatoms; R1 is selected from one of O and NSO2R0, R0 is a monovalent hydrocarbon group which may or may not contain heteroatoms; R2 is a monovalent hydrocarbon group which may or may not contain heteroatoms and may or may not contain heteroatoms.
[0010] In a possible implementation, the salt has a structure shown in Formula 2:
[0011]
[0012] In Formula 2, R3, R4, and R5 are independently selected from monovalent hydrocarbon groups having 1 to 20 carbon atoms which may or may not contain heteroatoms, m and n are independently selected from integers of 0 to 5, and o is an integer of 0 to 4; when m is greater than or equal to 2, at least two of the m R3s may be connected to each other to form a ring or not, when n is greater than or equal to 2, at least two of the n R4s may be connected to each other to form a ring or not, and when o is greater than or equal to 2, at least two of the o R5s may be connected to each other to form a ring or not.
[0013] In a possible implementation, R3, R4, and R5 are independently selected from monovalent hydrocarbon groups having 1 to 10 carbon atoms.
[0014] In a possible implementation manner, m and n are independently selected from integers of 1 to 3, and o is 0.
[0015] In one possible implementation, X is oxygen.
[0016] In a possible implementation, R1 is oxygen, and R2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms and substituted with at least one fluorine atom.
[0017] In a possible implementation, the salt has a structure shown in Formula 2-1 or Formula 2-2:
[0018]
[0019] The second aspect of the present application provides a method for preparing a salt, comprising the following steps:
[0020] Step 1: reacting the compound of formula 3 with the compound of formula 4 under anhydrous and oxygen-free conditions to obtain a compound of formula 5. The reaction process is as follows:
[0021]
[0022] In formulae 3 to 5, R3, R4, and R5 are independently selected from hydrocarbon groups having 1 to 20 carbon atoms which may contain heteroatoms, m and n are independently selected from integers of 0 to 5, and o is an integer of 0 to 4;
[0023] Step 2: reacting the compound represented by Formula 5 with the compound represented by Formula 6 to obtain the salt represented by Formula 2. The reaction process is as follows:
[0024]
[0025] In formula 6, X is a divalent linking group, L1 is selected from a single bond, a divalent hydrocarbon group with 1 to 20 carbon atoms that may contain heteroatoms; R1 is selected from one of O and NSO2R0, R0 is a hydrocarbon group with or without heteroatoms; R2 is a monovalent hydrocarbon group with 1 to 20 carbon atoms that may contain heteroatoms.
[0026] In a possible implementation, in step 1, the conditions for carrying out the reaction include: first reacting at a reaction temperature of -40°C to 0°C for 1 to 5 hours, and then raising the temperature to 23 to 28°C for 8 to 12 hours.
[0027] In a possible implementation, in step 2, the conditions for carrying out the reaction include: first reacting at a reaction temperature of -20°C to 0°C for 2 to 8 hours, and then raising the temperature to 23 to 28°C for 8 to 12 hours.
[0028] The third aspect of the present application provides a chemically amplified resist composition, comprising any of the above-mentioned salts, and also comprising an acid deprotection resin and a solvent.
[0029] In a possible implementation, the mass of the salt is 0.01% to 2% of the total mass of the chemically amplified resist composition.
[0030] The present application provides a monofluoro-substituted olefin sulfonate having an inner salt structure, wherein the inner salt structure helps to increase the polarity and steric hindrance of the salt, and the monofluoro-substituted olefin sulfonate structure has weaker acidity than conventional difluorosulfonate. On the basis of being able to cause the unstable groups of the resin acid to fall off, the diffusion coefficient of the acid generated is low, the diffusion performance is better controlled, and it helps to improve the exposure energy margin.
[0031] The fourth aspect of the present application provides the application of the chemically amplified resist composition as described in the third aspect of the present application in the field of patterning. The resist composition can be applied to semiconductor patterning processes to obtain high-quality patterns and improve the preparation precision and preparation efficiency of components.
[0032] A fifth aspect of the present application provides a patterning method, comprising:
[0033] Applying the chemically amplified resist composition described in the third aspect of the present application on a substrate to form a resist layer on the substrate;
[0034] exposing the resist layer through a mask;
[0035] The exposed resist layer is baked and developed with a developer to form a patterned thin film on the substrate.
[0036] The patterning method provided in the embodiment of the present application can be applied to the patterning process of the semiconductor manufacturing process by adopting a chemically amplified resist composition containing a specific structural salt, and it is easier to obtain high-quality small-size patterns.
[0037] The sixth aspect of the present application provides a patterned film, which is formed by the chemically amplified resist composition described in the third aspect of the present application, or the patterned film is obtained by the patterning method described in the fifth aspect of the present application. The patterned film can be used as a high-precision mask in the semiconductor patterning process, and the pattern of the patterned film can be transferred to a substrate such as a silicon wafer by etching to form a preset pattern on the substrate.
[0038] The seventh aspect of the present application provides a patterned substrate, which includes a substrate and a patterned film arranged on the substrate, and the patterned film is formed by the chemically amplified resist composition described in the third aspect of the present application, or is obtained by the patterning method described in the fifth aspect of the present application.
[0039] The present application also provides an electronic component, which is manufactured using the patterned film described in the sixth aspect of the present application or the patterned substrate described in the seventh aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1The H NMR spectrum of the inner salt provided in Example 1 of the present application;
[0041] Figure 2 The NMR F spectrum of the inner salt provided in Example 1 of the present application;
[0042] Figure 3 The H NMR spectrum of the inner salt provided in Example 2 of the present application;
[0043] Figure 4 This is the nuclear magnetic resonance F spectrum of the inner salt provided in Example 2 of the present application. DETAILED DESCRIPTION
[0044] The terms used in the implementation section of this application are only used to explain the specific embodiments of this application and are not intended to limit this application.
[0045] Chemically amplified photoresists mainly include polymer resins and photoacid generators (PAGs). The photoacid generator generates acid when irradiated by active light or radiation, and the main chain or branched chain of the polymer resin in the exposed or irradiated part reacts with the generated acid and is decomposed or cross-linked in a so-called "post-exposure baking" (PEB) manner, so that the polarity of the polymer resin is changed. This change in polarity causes a solubility difference in the developing solution between the irradiated exposed area and the unexposed area, thereby forming a positive or negative image of the mask on the substrate. Each photochemically generated catalyst molecule can promote many solubility conversion reaction events, and the initial exposure dose is "amplified" by a subsequent series of chemical reaction events.
[0046] Energy Latitude (EL) refers to the maximum allowable deviation of exposure energy within the allowable range of line width variation. While traditional photoacid generators can improve resolution and pattern roughness, their exposure energy latitude (EL) is generally poor, and there is room for improvement.
[0047] In order to solve the above technical problems, in a first aspect, an embodiment of the present application provides a salt having a structure shown in Formula 1:
[0048]
[0049] In Formula 1, M1 is selected from a substituted or unsubstituted first cyclic group, the first cyclic group includes N1 substituted or unsubstituted cyclic groups, N1≥1, when N1=1, the cyclic group is a benzene ring, when N1>1, at least one cyclic group among the N1 cyclic groups is a benzene ring; M2 is selected from a substituted or unsubstituted second cyclic group, the second cyclic group includes N2 substituted or unsubstituted cyclic groups, N2≥1, when N2=1, the cyclic group is a benzene ring, when N2>1, at least one cyclic group among the N2 cyclic groups is a benzene ring; M3 is selected from a substituted or unsubstituted third cyclic group, the third cyclic group includes N3 substituted or unsubstituted cyclic groups, N3≥1, when N3=1, the cyclic group is a benzene ring, when N3>1, at least one cyclic group among the N3 cyclic groups is a benzene ring;
[0050] Q1, Q2, and Q3 are independently a single bond, a heteroatom, or a divalent hydrocarbon group with 1 to 20 carbon atoms which may or may not contain heteroatoms; X is a divalent linking group; L1 is selected from a single bond, or a divalent hydrocarbon group with 1 to 20 carbon atoms which may or may not contain heteroatoms; R1 is selected from one of O and NSO2R0, R0 is a monovalent hydrocarbon group which may or may not contain heteroatoms; R2 is a monovalent hydrocarbon group which may or may not contain heteroatoms and may or may not contain heteroatoms.
[0051] The salt of the structure shown in Formula 1 provided in the present application has an inner salt structure and is a monofluoro-substituted olefin sulfonate. The inner salt structure helps to increase the polarity and steric hindrance of the salt, and the monofluoro-substituted olefin sulfonate structure has weaker acidity than the conventional difluorosulfonate. The salt can be used as a photoacid generator. On the basis of being able to cause the acid-labile groups in the resin to fall off, it helps to reduce the diffusion coefficient of the acid and improve the exposure energy margin.
[0052] In the structure shown in Formula 1 defined in the present application, the first cyclic group M1, the second cyclic group M2, and the third cyclic group M3 each include at least one cyclic group. When M1, M2, and M3 each include only one cyclic group, the cyclic group is a substituted or unsubstituted benzene ring. When M1, M2, and M3 each include two or more cyclic groups, they include at least one substituted or unsubstituted benzene ring, and the other cyclic group can be a substituted or unsubstituted aromatic (hetero) ring or (hetero) cyclic hydrocarbon group. Two or more cyclic groups can be connected by fusion or by groups.
[0053] The first cyclic group, the second cyclic group and the third cyclic group can be connected to each other through a Q group (specifically Q1, Q2, or Q3), and form a ring with the central sulfur atom, which are respectively recorded as M4 ring, M5 ring, and M6 ring (see the above formula 1). Specifically, when Q1, Q2, and Q3 are present, Q1, Q2, and Q3 are independently a single bond, a heteroatom, or a divalent hydrocarbon group with 1 to 20 carbon atoms containing or not containing heteroatoms; when Q1, Q2, and Q3 are independently a single bond, it means that the first cyclic group, the second cyclic group, and the third cyclic group are connected by a single bond; heteroatoms refer to atoms other than carbon and hydrogen, such as nitrogen (N), oxygen (O), sulfur (S), phosphorus (P), chlorine (Cl), bromine (Br), iodine (I), etc. When Q1, Q2, and Q3 do not exist, it means that the first cyclic group, the second cyclic group, and the third cyclic group are independent of each other, and accordingly, the M4 ring, the M5 ring, and the M6 ring do not exist. For example, the structure of Formula 1 can be
[0054] In the present application, "monovalent hydrocarbon group" refers to a monovalent group corresponding to a saturated or unsaturated hydrocarbon containing a corresponding number of carbon atoms. For example, it can be a saturated hydrocarbon group, an olefin group, an alkynyl group, an aromatic hydrocarbon group or any combination thereof; it can be linear, branched, cyclic or any combination thereof. Exemplarily, a monovalent hydrocarbon group may include, but is not limited to, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, allyl, isoprenyl, 2-butenyl, 2-hexenyl, propargyl, butynyl, phenyl (-C6H5), naphthyl, etc. A divalent hydrocarbon group refers to a group formed after two hydrogen atoms bound to a carbon atom in a hydrocarbon substance are removed, that is, a divalent hydrocarbon group is a group formed after one hydrogen atom bound to a carbon atom in its corresponding monovalent hydrocarbon group is removed. Exemplarily, a divalent hydrocarbon group may be a methylene group (-CH2-), an ethylene group (-CH2CH2-), a phenylene group (-C6H4-), etc. In addition, the carbon atoms and / or hydrogen atoms in the above-mentioned monovalent or divalent hydrocarbon group may be replaced by one or more heteroatoms. Heteroatoms refer to atoms other than carbon and hydrogen, such as nitrogen (N), oxygen (O), sulfur (S), phosphorus (P), chlorine (Cl), bromine (Br), iodine (I), etc.
[0055] X represents a linking group, and specifically may be a heteroatom, such as oxygen (O), sulfur (S), and the like.
[0056] When L1 is a single bond, it means that X is directly connected to the carbon atom on the double bond.
[0057] In a possible implementation, when N1, N2, and N3 are all 1, the salt has a structure shown in Formula 2:
[0058]
[0059] In Formula 2, R3, R4, and R5 are independently selected from monovalent hydrocarbon groups having 1 to 20 carbon atoms which may contain heteroatoms, m and n are independently selected from integers of 0 to 5, and o is an integer of 0 to 4.
[0060] When m, n, and o are zero, it means that M1, M2, and M3 only include unsubstituted benzene rings, and any two adjacent benzene rings can exist independently, or form a ring with the sulfur atom and the carbon atom on the benzene ring through the Q group, for example:
[0061]
[0062] When m, n, and o are independently integers greater than or equal to 1, the substituents R3, R4, and R5 are independently selected from hydrocarbon groups having 1 to 20 carbon atoms with or without heteroatoms, and their positions on the benzene ring are not further limited.
[0063] In another possible implementation, when at least one of N1, N2, and N3 is an integer greater than 1, it means that at least one of the first cyclic group M1, the second cyclic group M2, and the third cyclic group M3 includes two or more cyclic groups, for example, aromatic (hetero) rings or (hetero) cyclic hydrocarbon groups, and adjacent cyclic groups can be connected by fusion or single bonds. Exemplarily, the above M1, M2, and M3 are selected from the groups corresponding to the following compounds:
[0064]
[0065] Wherein, when Q1, Q2, Q3 do not exist, M1, M2, M3 are specifically the following groups:
[0066]
[0067] In addition, when at least one of N1, N2, and N3 is an integer greater than 1, it can be connected to an adjacent cyclic group or a sulfur atom to form a ring through any cyclic group. For example, the structure on the left side of X in Formula 1 can be any of the following structures:
[0068]
[0069] In a possible implementation, R3, R4, and R5 are independently selected from monovalent hydrocarbon groups having 1 to 10 carbon atoms.
[0070] In a possible implementation manner, m and n are independently selected from integers of 1 to 3, and o is 0.
[0071] In one possible implementation, X is oxygen.
[0072] In a possible implementation, R1 is oxygen, and R2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms and substituted with at least one fluorine atom.
[0073] In a possible implementation, the salt is a salt represented by Formula 2-1 or Formula 2-2:
[0074]
[0075]
[0076] The salt having the structure shown in Formula 2 provided in the present application can be prepared by referring to the following preparation method, which specifically comprises the following steps:
[0077] Step 1: reacting the compound represented by Formula 3 and the compound represented by Formula 4 under anhydrous and oxygen-free conditions to obtain the compound represented by Formula 5. The reaction process is as follows:
[0078]
[0079] In formulae 3 to 5, R33, R4, and R5 are independently selected from monovalent hydrocarbon groups having 1 to 20 carbon atoms which may or may not contain heteroatoms, m and n are independently selected from integers of 0 to 5, and o is an integer of 0 to 4;
[0080] Step 2: reacting the compound of formula 5 with the compound of formula 6 to obtain the salt of formula 2. The reaction process is as follows:
[0081]
[0082] In formula 6, X is a divalent linking group, L1 is selected from a single bond, a divalent hydrocarbon group with 1 to 20 carbon atoms that may contain heteroatoms; R1 is selected from one of O and NSO2R0, R0 is a hydrocarbon group with or without heteroatoms; R2 is a monovalent hydrocarbon group with 1 to 20 carbon atoms that may contain heteroatoms.
[0083] In a possible implementation, in step 1, the reaction temperature is controlled at -40°C to 0°C for 1 to 5 hours, and then the temperature is increased to 23 to 28°C for 8 to 12 hours.
[0084] In a possible implementation, the reaction shown in step 1 is carried out in the presence of trimethylsilyl bromide (TMSBr), and the solvent is tetrahydrofuran (THF).
[0085] In a possible implementation, in step 2, the reaction temperature is controlled at -20°C to 0°C for 2 to 8 hours, and then the temperature is increased to 23 to 28°C for 8 to 12 hours.
[0086] In a possible implementation, the reaction shown in step 2 is carried out in the presence of NaH, and the solvent is THF.
[0087] The present application also provides a chemically amplified resist composition, comprising any of the above-mentioned salts.
[0088] Based on the salt provided in the first aspect of the present application, the chemically amplified resist composition comprising the salt has lower acid diffusion, which helps to improve the exposure energy margin of the etchant resistance layer formed by the resist composition.
[0089] In a possible implementation, the chemically amplified resist composition further comprises an acid deprotection resin (i.e., a resin containing an acid-labile protection group) and a solvent. The acid deprotection resin can be selected from a substance having a multi-monomer copolymer structure; the solvent is used to disperse the acid deprotection resin and the photoacid generator to form a liquid substance with good fluidity, which can be coated on the substrate surface by rotation.
[0090] In a possible implementation, the mass of the salt is 0.01% to 2% of the total mass of the chemically amplified resist composition, the mass of the acid deprotection resin is 2.0% to 10.0% of the total mass of the chemically amplified resist composition, and the remainder is solvent.
[0091] In a possible implementation, the chemically amplified resist composition further includes a quencher, which helps to improve the resolution of the material to the light source and reduce the impact of acids and bases in the environment on the material. The quencher can be selected from alkaline quenchers and radiation-sensitive quenchers. Further, the radiation-sensitive quencher is a photodecomposable base.
[0092] In a possible implementation, the chemically amplified resist composition further includes additives to change certain properties of the composition, which can be added as needed.
[0093] The chemically amplified resist composition provided in the present application can be used in the field of patterning, for example, to form a patterned film on the surface of a substrate. In addition, the above-mentioned salt provided in the present application can be used as a photosensitive acid-generating component (i.e., as a photoacid generator), and can also decompose and generate acid when heated, and can also be used in other fields that require acid generation, such as photocurable materials, thermal curable materials, etc.
[0094] The present application also provides a patterning method, comprising:
[0095] (1) coating the chemically amplified resist composition provided by the present application on a substrate to form a resist layer on the substrate;
[0096] (2) exposing the resist layer through a mask;
[0097] (3) baking the exposed resist layer and developing it with a developer to form a patterned thin film on the substrate.
[0098] In step (1), the substrate can be selected according to specific needs, for example, it can be a silicon wafer, or a silicon wafer covered with other coatings; the other coatings can be a bottom anti-reflective coating, a dielectric layer, a metal layer, or a modified layer.
[0099] The coating method of the chemically amplified resist composition includes, but is not limited to, one or more of spin coating, roller coating, flow coating, dip coating, spray coating, blade coating, etc. The thickness of the wet film applied can be adjusted according to the thickness of the dry resist layer to be formed. Generally, after applying the chemically amplified resist composition, pre-baking is also performed to minimize the solvent content in the composition.
[0100] In step (2), the exposure source used for exposure can be ordinary ultraviolet light (200nm-400nm), KrF excimer laser (248nm), ArF excimer laser (193nm), extreme ultraviolet light with a wavelength of 1nm-15nm, X-rays (such as a wavelength of 1nm-15nm), or electron beams, etc.
[0101] During exposure, a mask with a predetermined pattern is placed above the resist layer, and an exposure source selectively exposes the resist layer through the mask. After the patterned material film layer is selectively exposed, the salt as a photoacid generator in the exposed area decomposes to generate acid, so that the exposed area and the non-exposed area have a solubility difference in the developer during the post-exposure baking process. Since the dry etchant layer of the resist composition containing the salt provided by the present application has low acid diffusion, the exposure energy margin of the etchant layer is relatively wide.
[0102] In step (3), the baking after exposure promotes the acid-deprotected resin in the exposed area of the acid-catalyzed photoresist layer generated during the exposure process to undergo deprotection of the acid-labile groups, thereby changing the polarity of the resin. This change in polarity results in a difference in the solubility of the developer between the exposed area and the unexposed area of the resist layer, thereby forming a positive image or a negative image of the mask on the substrate. If the exposed area of the resist layer is washed away after being treated with the developer, the development is positive development, forming a positive pattern; if the unexposed area of the resist layer is washed away after being treated with the developer, the development is negative development, forming a negative pattern.
[0103] In some embodiments of the present application, after the above step (3), the following step (4) is also included: etching the substrate using the patterned film as a mask to transfer the pattern of the patterned film to the substrate to obtain a patterned substrate.
[0104] During the etching process, the patterned film formed by the chemically amplified resist composition can selectively protect the substrate material located thereunder. After etching under certain conditions, the substrate material not protected by the patterned film can be etched away, and the substrate material protected by the patterned film can be retained, and finally a pattern is formed on the substrate material, that is, the pattern of the patterned film is transferred to the substrate. It is understandable that the patterned film generally needs to be removed. That is, the patterned film generally does not exist on the patterned substrate. Subsequently, other functional layers can be prepared on the patterned substrate.
[0105] The above-mentioned patterning method provided in the embodiment of the present application can be applied to the patterning process of the semiconductor preparation process by adopting the chemically amplified resist composition provided in the embodiment of the present application, and it is easier to obtain high-quality small-size patterns, which is conducive to the development of semiconductor devices towards high integration and high precision.
[0106] The embodiment of the present application also provides a patterned film, which is formed by using the chemically amplified resist composition described in the embodiment of the present application, or is obtained by using the patterning method described above.
[0107] The patterned film can be used as a high-precision mask in the patterning process of manufacturing semiconductor devices, and the pattern of the patterned film can be transferred to a substrate such as a silicon wafer by etching to form a preset pattern on the substrate. Since the chemically amplified resist composition provided in the embodiment of the present application has high exposure sensitivity and a high exposure energy margin, the pattern of the patterned film obtained by the patterning process has the advantages of high resolution and low edge roughness.
[0108] The embodiment of the present application also provides a patterned substrate, which includes: a substrate and a patterned film arranged on the substrate, and the pattern on the patterned film is formed using the chemically amplified resist composition of the embodiment of the present application or obtained using the above-mentioned patterning method.
[0109] The patterned substrate can be used in the preparation of electronic components such as chips, improving the manufacturing accuracy and quality of the devices, thereby improving the performance of the electronic components.
[0110] The embodiment of the present application also provides an electronic component, which is manufactured using the patterned film or patterned substrate provided above. The method for manufacturing the electronic component includes the patterning method described above in the present application.
[0111] The electronic components may include chips, etc. In the process of preparing the chip, after completing the patterning process for forming the patterned film, other functional layers may be prepared.
[0112] The salts and compositions provided in this application are described in detail below in conjunction with specific examples:
[0113] Example 1
[0114] The salt provided in this embodiment has a structure as shown in Formula 2-1:
[0115]
[0116] The preparation method of the salt provided in this embodiment comprises the following steps:
[0117] Step 1, in a 500mL three-necked flask, at -40°C, under anhydrous and oxygen-free conditions, diphenyl sulfoxide (9.45g, 30mmol, 1.0eq.) was dissolved in anhydrous tetrahydrofuran (50mL), p-fluorophenylmagnesium bromide (1.0M, 75mL, 75mmol, 2.5eq.) was added dropwise, followed by stirring for 15 minutes, and then trimethylsilyl bromide (TMSBr) (9.90mL, 3.83g, 75mmol, 2.5eq.) was slowly added dropwise (10min), followed by reaction at -20°C for 3h, and then warmed to room temperature for reaction overnight.
[0118] Pour the reaction solution into HBr ice water, adjust the pH to pH=1, dilute with water, extract with dichloromethane (DCM) 3 times, combine the organic phases, wash with saturated brine, dry, evaporate to dryness, and obtain a viscous crude product. Add ether (the product is insoluble), stir and shake well, and carefully pour off the ether solution, taking care not to lose the product. Repeat 2-3 times, and vacuum dry to obtain the pure product sulfonium2, a powdery solid. Seal, protect from light, and store in a dry place. The yield is about 70%.
[0119]
[0120] Step 2: In a 250 mL three-necked flask, add 4.79 g sulfonium 2 and 2.52 g sodium 1,1,3,3,3-pentafluoro-2-hydroxy-propane sulfonate, and dissolve in 20 mL anhydrous THF. At 0°C, slowly add 750 mg NaH powder and react for 5 h, then warm to room temperature and continue to react for 12 h.
[0121] The reaction was quenched with 1% HCl, extracted with dichloromethane (DCM) three times, the organic phases were combined, washed with saturated brine, dried, evaporated to dryness, and recrystallized with methanol, dichloromethane, and ether to obtain the pure product with a yield of about 50%.
[0122]
[0123] The prepared salt was dissolved in CDCl3 and subjected to NMR detection. The NMR H and F spectra of the salt were as follows: Figure 1-Figure 2 As shown, the structure of the salt can be confirmed.
[0124] Example 2
[0125] The salt provided in this embodiment has a structure as shown in Formula 2-2:
[0126]
[0127] The preparation method of the salt provided in this embodiment comprises the following steps:
[0128] Step 1, in a 500mL three-necked flask, at -40°C, under anhydrous and oxygen-free conditions, di(p-tert-butylphenyl)sulfoxide (9.45g, 30mmol, 1.0eq.) was dissolved in anhydrous tetrahydrofuran (50mL), p-fluorophenylmagnesium bromide (1.0M, 75mL, 75mmol, 2.5eq.) was added dropwise, followed by stirring for 15 minutes, and then trimethylsilyl bromide (TMSBr) (9.90mL, 3.83g, 75mmol, 2.5eq.) was slowly added dropwise (10min), followed by reaction at -40°C for 3h, and then warmed to room temperature for reaction overnight.
[0129] Pour the reaction solution into HBr ice water, adjust the pH to pH=1, dilute with water, extract with dichloromethane (DCM) 3 times, combine the organic phases, wash with saturated brine, dry, evaporate to dryness, and obtain a viscous crude product. Add ether (the product is insoluble), stir and shake well, and carefully pour off the ether solution, taking care not to lose the product. Repeat 2-3 times, and vacuum dry to obtain the pure product sulfonium2, a powdery solid. Seal, protect from light, and store in a dry place. The yield is about 70%.
[0130]
[0131] Step 2: In a 250 mL three-necked flask, add 4.79 g sulfonium 2 and 2.52 g sodium 1,1,3,3,3-pentafluoro-2-hydroxy-propane sulfonate, and dissolve in 20 mL anhydrous THF. At 0°C, slowly add 750 mg NaH powder and react for 5 h, then warm to room temperature and continue to react for 12 h.
[0132] The reaction was quenched with 1% HCl, extracted with dichloromethane (DCM) three times, the organic phases were combined, washed with saturated brine, dried, evaporated to dryness, and recrystallized with methanol, dichloromethane, and ether to obtain the pure product PAG-2 with a yield of about 50%.
[0133]
[0134] The prepared salt was dissolved in CDCl3 and subjected to NMR detection. The NMR H and F spectra of the salt were as follows: Figure 3-Figure 4 As shown, the structure of the salt can be confirmed.
[0135] Comparative Example 1
[0136] The structure of the salt used in this comparative example is shown in Formula 2-3:
[0137]
[0138] The photoacid generator provided in Example 2 and Comparative Example 1 was combined with an acid-deprotectable resin, a quencher (i.e., a photodegradable base), and a solvent to prepare a chemically amplified resist composition. After the composition was coated to form a dry film layer, it was exposed using a 193nm ArFi excimer laser, and the EL was calculated. The results are shown in Table 1.
[0139] Among them, the structure of the photodecomposable base is shown below:
[0140]
[0141] The structure of the acid deprotectable resin is shown below:
[0142]
[0143] Table 1 EL after exposure of the chemically amplified resist compositions provided in Example 2 and Comparative Example 1
[0144] EL(%) Improvement percentage (%) Example 2 29.16% 18.5% Comparative Example 1 24.61% /
[0145] It can be seen from Table 1 that the salt provided in the present application helps to ensure that the chemically amplified resist composition has a higher EL value.
[0146] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the embodiments of the present application, rather than to limit them. Although the embodiments of the present application have been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A salt, characterized in that The salt has a structure shown in Formula 1: In Formula 1, M1 is selected from a substituted or unsubstituted first cyclic group, the first cyclic group includes N1 substituted or unsubstituted cyclic groups, N1 ≥ 1, when N1 = 1, the cyclic group is a benzene ring, when N1 > 1, at least one cyclic group in the N1 cyclic groups is a benzene ring; M2 is selected from a substituted or unsubstituted second cyclic group, the second cyclic group includes N2 substituted or unsubstituted cyclic groups, N2 ≥ 1, when N2 = 1, the cyclic group is a benzene ring, when N2 > 1, at least one cyclic group in the N2 cyclic groups is a benzene ring; M3 is selected from a substituted or unsubstituted third cyclic group, the third cyclic group includes N3 substituted or unsubstituted cyclic groups, N3 ≥ 1, when N3 = 1, the cyclic group is a benzene ring, when N3 > 1, at least one cyclic group in the N3 cyclic groups is a benzene ring; Q1, Q2, and Q3 are independently a single bond, a heteroatom, a divalent hydrocarbon group with 1 to 20 carbon atoms that may or may not contain heteroatoms, or do not exist; X is a divalent linking group; L1 is selected from a single bond, a divalent hydrocarbon group with 1 to 20 carbon atoms that may or may not contain heteroatoms; R1 is selected from one of O and NSO2R0, R0 is a monovalent hydrocarbon group that may or may not contain heteroatoms; R2 is a monovalent hydrocarbon group with 1 to 20 carbon atoms that may or may not contain heteroatoms.
2. The salt according to claim 1, characterized in that The salt has a structure shown in Formula 2: In Formula 2, R3, R4, and R5 are independently selected from monovalent hydrocarbon groups having 1 to 20 carbon atoms which may or may not contain heteroatoms, m and n are independently selected from integers of 0 to 5, and o is an integer of 0 to 4; when m is greater than or equal to 2, at least two of the m R3s may be connected to each other to form a ring or not, when n is greater than or equal to 2, at least two of the n R4s may be connected to each other to form a ring or not, and when o is greater than or equal to 2, at least two of the o R5s may be connected to each other to form a ring or not.
3. The salt according to claim 2, characterized in that R3, R4, and R5 are independently selected from monovalent hydrocarbon groups having 1 to 10 carbon atoms.
4. The salt according to claim 2 or 3, characterized in that m and n are independently selected from integers of 1 to 3, and o is 0.
5. The salt according to claim 1 or 2, characterized in that X is oxygen.
6. The salt according to claim 1 or 2, characterized in that R1 is oxygen, and R2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms substituted with at least one fluorine atom.
7. The salt according to any one of claims 1 to 6, characterized in that The salt has a structure shown in Formula 2-1 or Formula 2-2:
8. A method for preparing salt, characterized in that: The steps include: Step 1: reacting the compound of formula 3 with the compound of formula 4 under anhydrous and oxygen-free conditions to obtain the compound of formula 5. The reaction process is as follows: In formulas 3 to 5, R3, R4, and R5 are independently selected from monovalent hydrocarbon groups having 1 to 20 carbon atoms which may contain heteroatoms, m and n are independently selected from integers of 0 to 5, and o is an integer of 0 to 4; Step 2: reacting the compound represented by Formula 5 with the compound represented by Formula 6 to obtain the salt represented by Formula 2. The reaction process is as follows: In formula 6, X is a divalent linking group, L1 is selected from a single bond, a divalent hydrocarbon group with 1 to 20 carbon atoms that may contain heteroatoms; R1 is selected from one of O and NSO2R0, R0 is a hydrocarbon group with or without heteroatoms; R2 is a monovalent hydrocarbon group with 1 to 20 carbon atoms that may contain heteroatoms.
9. The preparation method according to claim 8, characterized in that In step 1, the reaction conditions include: first reacting at a reaction temperature of -40°C to 0°C for 1 to 5 hours, and then raising the temperature to 23 to 28°C for 8 to 12 hours.
10. The preparation method according to claim 8, characterized in that In step 2, the reaction conditions include: first reacting at a reaction temperature of -20°C to 0°C for 2 to 8 hours, and then raising the temperature to 23 to 28°C for 8 to 12 hours.
11. A chemically amplified resist composition, characterized in that: The chemically amplified resist composition comprises the salt according to any one of claims 1 to 7 or the salt prepared by the preparation method according to any one of claims 8 to 10, and further comprises an acid deprotecting resin and a solvent.
12. The chemically amplified resist composition according to claim 11, wherein The mass of the salt is 0.01% to 2% of the total mass of the chemically amplified resist composition.
13. The chemically amplified resist composition according to claim 11 or 12, characterized in that The chemically amplified resist composition further includes a quencher.
14. Use of the chemically amplified resist composition according to any one of claims 11 to 13 in the field of patterning.
15. A patterning method, characterized in that: include: coating the chemically amplified resist composition according to any one of claims 11 to 13 on a substrate to form a resist layer on the substrate; exposing the resist layer through a mask; The exposed resist layer is baked and developed with a developer to form a patterned thin film on the substrate.
16. A patterned film, characterized in that: The patterned film is formed by the chemically amplified resist composition according to any one of claims 11 to 13, or the patterned film is obtained by the patterning method according to claim 15.
17. A patterned substrate, characterized in that The invention comprises a substrate and a patterned film arranged on the substrate, wherein the patterned film is formed by the chemically amplified resist composition according to any one of claims 11 to 13, or is obtained by the patterning method according to claim 15.
18. An electronic component, characterized in that: The method is prepared by using the patterned film according to claim 16 or the patterned substrate according to claim 17.