Degradable polymer water-absorbent resin and preparation method thereof
By compounding soy protein isolate powder with acrylic acid monomers and using easily hydrolyzable group cross-linking agents, the degradability and liquid-absorbing performance of the polymer water-absorbent resin are improved, and the problem of poor degradability of polyacrylic acid resins is solved. It is suitable for Disposable sanitary products.
Patent Information
- Application Number
- CN202410916181.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
AI Technical Summary
Existing polyacrylic polymer water-absorbent resins have poor degradability, insufficient liquid absorption rate and water retention, making it difficult to meet the needs of disposable sanitary products.
By compounding soy protein isolate powder with acrylic acid monomer, and using macromolecular cross-linking agents containing easily hydrolyzable groups, the synthesis process and initiating system are adjusted to improve the degradability and super-absorbency of the resin.
The degradability of polymer water-absorbent resin has been improved. The absorption rate of deionized water reaches 1765g/g, the absorption rate of physiological saline is 101g/g, the centrifugal water retention rate is 1533g/g, and the degradation rate reaches 60.37% in 60 days. It is suitable for disposable use. sanitary napkins and diapers.
Smart Images

Figure CN118725210A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer water-absorbing resin synthesis, and in particular relates to a degradable polymer water-absorbing resin and a preparation method thereof. Background Art
[0002] Polymer water-absorbent resin is a new type of polymer material with excellent water absorption and water retention. It contains many strong hydrophilic groups such as carboxyl, amine, and sulfonic acid groups, and has a certain degree of crosslinking. It itself is insoluble in water and any organic agent. Because this type of material has a unique three-dimensional spatial network structure, it can absorb hundreds or even thousands of times its own weight of water through hydration and swell into a gel state. Water will not precipitate under a certain range of pressure. The resin after absorbing water can restore its water absorption performance after drying, so it has important application prospects in many fields. However, most of the widely used hydrogel materials are prepared by petroleum-based polymer materials such as polyvinyl alcohol (PVA), polyacrylic acid (PAA), and polyacrylamide (PAM). Not only are there problems of non-degradability, but there are also potential hidden dangers in terms of safety in use. Natural polymer materials represented by polysaccharides and proteins have the advantages of wide sources, diverse chemical compositions, good biocompatibility and biodegradability. Hydrogels based on natural polymers can overcome the problems brought by petroleum-based polymer hydrogels and have become a hot spot in current research and application.
[0003] Soy protein isolate (SPI) is a renewable natural polymer with good biocompatibility and biodegradability, and contains multiple active side groups such as amino, carboxyl, hydroxyl and sulfhydryl, etc. These groups make it have good water absorption, water retention and swelling, and are almost unaffected by temperature, and the highest water retention capacity reaches 14g water / g protein. In addition, these active groups can also react chemically with many substances, and are a kind of material with multiple reactivity. Patent CN200410077759 "modified soybean protein isolate based super absorbent and preparation method thereof" discloses a modified soybean protein isolate synthetic hydrogel for preparing super absorbent, but the super absorbent resin obtained by this method has a deionized water absorption rate of only 538g / g, and the salt water absorption rate is up to 66.7g / g, which has a problem of low liquid absorption rate.
[0004] In addition to graft copolymerization of natural polymers to obtain biodegradability, chemical modification can also increase the biodegradability of polymer absorbent resins. This method requires the presence of certain non-biochemical mechanisms, so that the polymer is first decomposed into relatively small polymer molecules (relative molecular weight M is reduced to less than 1500g / mol) under the action of external non-biochemical factors (such as thermal decomposition, hydrolysis or chemical decomposition). The simplest and most feasible method to achieve CC skeleton decomposition is to introduce a "weak bond" on the polymer main chain so that the skeleton can be degraded by non-biological effects (such as hydrolysis). During the polymerization process, the main chain is connected by using a cross-linking agent containing ester bonds, ether bonds, epoxy and other easy-to-hydrolyze cross-linking agents, which can play a role in improving the degradability of the molecule. Patent CN115109201A "A cross-linking agent for degradable hydrogel and a degradable polyacrylamide hydrogel based on a cross-linking agent and its preparation method and use" discloses a synthesis method of a cross-linking agent for degradable hydrogel, so that the cross-linking agent breaks the gel under alkaline conditions, thereby achieving the degradability of the gel. However, this method cannot guarantee the degradation rate of the molecules, especially the main chain of the polyacrylamide molecule is difficult to degrade, which makes this method have certain defects. Patent CN116874690A "A degradable antibacterial composite super absorbent resin and its preparation method" discloses that silk fibroin powder is compounded with acrylic acid and acrylamide monomers to improve the water absorption and degradability of the super absorbent resin, improving the problem that traditional acrylic super absorbent resins are non-degradable, but the absorbent resin obtained by this method has a low water absorption rate and insufficient degradation rate. Summary of the invention
[0005] Aiming at the problems of poor degradability, poor liquid absorption rate and poor water retention of current polyacrylic acid polymer water-absorbent resins, the present invention prepares a biodegradable polymer water-absorbent resin.
[0006] The purpose of the present invention is to provide a method for preparing a degradable polymer water-absorbent resin. The method greatly improves the degradability of the resin by compounding soy protein isolate powder with acrylic acid monomer and using a macromolecular cross-linking agent containing an easily hydrolyzed group, thereby improving the problem that traditional polyacrylic acid hydrogel is difficult to degrade.
[0007] The purpose of the present invention is to make the polymer resin degradable, and to make the resin super absorbent by adjusting the initiator system and the amount of the crosslinking agent, and adjusting the synthesis process. The polymer absorbent resin can be applied to the fields of disposable sanitary napkins and diapers / sheets.
[0008] The purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing a degradable polymer water-absorbing resin comprises the following steps:
[0010] (1) Weighing an appropriate amount of acrylic acid, and diluting it with a certain amount of deionized water to obtain a mixed solution 1;
[0011] (2) Weighing an appropriate amount of sodium hydroxide particles and dissolving them in an appropriate amount of deionized water to obtain a mixed solution 2;
[0012] (3) then adding the mixed solution 2 dropwise to the mixed solution 1 in an ice water bath, controlling the reaction heat during the neutralization process, to obtain a mixed solution 3;
[0013] (4) adding sodium dodecyl sulfate (SDS) and soy protein isolate powder (SPI) to a certain amount of deionized water, stirring at 60-90° C. to obtain a uniform solution, cooling to room temperature, and adjusting the pH with 0.1% NaOH solution to obtain a mixed solution 4;
[0014] (5) Mixing the mixed solution 3 and the mixed solution 4 to obtain a mixed solution 5, adding a crosslinking agent, and heating at 40-50° C. for 10-30 min, then adding an initiator system, evacuating the mixture, and introducing nitrogen to carry out a free radical polymerization reaction;
[0015] (6) After the reaction is completed, the product is dried and crushed to obtain the degradable polymer water-absorbent resin.
[0016] Furthermore, the acrylic acid in step (1) accounts for 25%-40% of the total mass of the mixed solution 5.
[0017] Furthermore, the concentration of acrylic acid in the mixed solution 1 in step (1) is 70%-85%.
[0018] Furthermore, the concentration of sodium hydroxide in the mixed solution 2 in step (2) is 20%-40%.
[0019] Furthermore, in step (3), the temperature of the reaction heat of the neutralization process is controlled to be 20-35°C.
[0020] Furthermore, the neutralization degree of carboxyl groups in the mixed solution 3 is 60%-80%.
[0021] Furthermore, in step (4), the mass ratio of SDS to SPI is 0.125-1.20; the mass of the soy protein isolate powder accounts for 0.01%-30% of the mass of the acrylic acid; and after cooling, the pH is adjusted to 6-10 with 0.1% NaOH solution.
[0022] Furthermore, the cross-linking agent in step (5) is one or more of pentaerythritol dimethacrylate, tetraethylene glycol diacrylate, poloxamer diacrylate, ethylene glycol diglycidyl ether and polyethylene glycol monomethyl ether acrylate; and the cross-linking agent in the mixed solution 5 accounts for 0.1‰-1.0‰ of the mass of acrylic acid.
[0023] Furthermore, the initiation system in step (5) comprises an initiator and a reducing agent, wherein the initiator is one or more of potassium persulfate or ammonium persulfate; the reducing agent is one or more of sodium sulfite or sodium bisulfite; and the initiator in the mixed solution 5 accounts for 0.5‰-2‰ of the mass of acrylic acid, and the reducing agent accounts for 0.5‰-2‰ of the mass of acrylic acid.
[0024] Furthermore, the initiation temperature of the free radical polymerization reaction in step (5) is 40-60° C., and the thermal initiation reaction time is 0.5-3 h.
[0025] Furthermore, the temperature of the free radical polymerization reaction in step (5) is 60-90° C., and the polymerization reaction time is 3-6 hours.
[0026] Furthermore, the drying temperature in step (6) is 70-110° C., and the drying time is 8-24 hours.
[0027] The degradable polymer water-absorbent resin of the present invention is prepared by the above method. The resin can absorb deionized water at a maximum rate of 1765 g / g, absorb 0.9% saline at a rate of 101 g / g, have a centrifugal water retention rate of 1533 g / g, and a degradation rate of 60 days of degradation of 60.37%.
[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0029] (1) The processing process of soy protein isolate is simplified. It does not need to be modified. It only needs to be mixed and heated with SDS and the pH of the system is appropriately adjusted. The operation is simple.
[0030] (2) Introducing soy protein isolate powder into the molecular chain of traditional polyacrylic acid super absorbent resin expands the raw material source of super absorbent resin and improves the biocompatibility and degradability of composite polyacrylic acid super absorbent resin, which is more environmentally friendly than pure petroleum-based polymer absorbent resin.
[0031] (3) Using a molecular cross-linking agent containing an easily hydrolyzed group, compared with the traditional N,N'-methylenebisacrylamide, expands the three-dimensional grid structure, which can not only improve the liquid absorption rate and water retention rate of the hydrogel, but also effectively improve its degradability. The cross-linking agent selected by the present invention contains a large number of ether bonds or ester bonds and other groups that are easily chemically hydrolyzed in the molecular structure, which is conducive to the degradation of the resin. In addition, the cross-linking agent of the present invention plays a role in connecting the molecular segments to each other. The size of the three-dimensional network structure of the resin affects its liquid absorption performance. The longer the molecular segment, the larger the resin grid and the better the liquid absorption performance. Therefore, the resin can be made super absorbent by adjusting the initiation system and the amount of the cross-linking agent, and adjusting the synthesis process at the same time.
[0032] (4) The degradable polymer water-absorbent resin prepared by the present invention does not require special equipment, the raw materials are cheap and easy to obtain, the sources are wide, and the preparation method is simple and easy to operate. The degradable polymer water-absorbent resin prepared by the present invention has broad application prospects in the field of disposable sanitary products such as diapers / sheets and sanitary napkins for women. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the infrared spectrum of the degradable polymer water-absorbent resin prepared in Example 1.
[0034] Figure 2 This is a scanning electron microscope image of the degradable polymer water-absorbent resin prepared in Example 5.
[0035] Figure 3 This is the mass change curve of the degradable polymer water-absorbent resin prepared in Example 5 after continuous degradation for 60 days. DETAILED DESCRIPTION
[0036] The present invention is further described below in conjunction with specific embodiments and drawings.
[0037] Example 1
[0038] 25 g of acrylic acid was weighed and diluted with 10 ml of water to obtain a mixed solution 1, 10.85 g of sodium hydroxide was dissolved in 35 ml of water to obtain a mixed solution 2, and the mixed solution 2 was added dropwise to the mixed solution 1 in an ice-water bath, and the temperature of the neutralization system was controlled to be maintained at 20-35° C. to obtain a mixed solution 3; 0.0013 g of sodium dodecyl sulfate (SDS) and 0.0025 of soy protein isolate powder (SPI) were added to 3 ml of deionized water, and stirred at 90° C. for 1 hour to obtain a uniform solution, and after cooling to room temperature, the pH was adjusted to 9.0 with a 0.1% NaOH solution to obtain a mixed solution 4; the mixed solution 3 and the mixed solution 4 were mixed to obtain a mixed solution 5, and 0.001 g of pentaerythritol dimethacrylate was added and co-heated at 45° C. for 10 minutes, and then 0.0125 g of potassium persulfate and 0.0125 g of sodium bisulfite were added, and then vacuum was evacuated and nitrogen was introduced to perform free radical polymerization. The reaction was carried out at this temperature for 1 hour, then the temperature was raised to 60°C for 1 hour, and finally the temperature was raised to 80°C for 2 hours. After the reaction was completed, the product was dried at 90°C for 18 hours and crushed to obtain the degradable polymer water-absorbing resin.
[0039] Example 2
[0040] Weigh 25g of acrylic acid and dilute it with 10ml of water to obtain mixed solution 1, dissolve 9.71g of sodium hydroxide with 32ml of water to obtain mixed solution 2, add mixed solution 2 dropwise to mixed solution 1 in an ice-water bath, control the temperature of the neutralization system to be maintained at 20-35°C, and obtain mixed solution 3; add 0.4g of sodium dodecyl sulfate (SDS) and 2.5g of soy protein isolate powder (SPI) to 20ml of deionized water, stir at 90°C for 1h to obtain a uniform solution, cool to room temperature, adjust the pH to 7.0 with 0.1% NaOH solution, and obtain mixed solution 4; mix mixed solution 3 and mixed solution 4 to obtain mixed solution 5, add 0.0025g of tetraethylene glycol diacrylate, heat at 45°C for 10min, then add 0.025g of ammonium persulfate and 0.025g of sodium bisulfite, evacuate and introduce nitrogen for free radical polymerization. React at this temperature for 1h, then heat to 60°C for 1h, and finally heat to 80°C for 2h. After the reaction is completed, the product is dried at 100° C. for 12 hours and crushed to obtain the degradable polymer water-absorbent resin.
[0041] Example 3
[0042] Weigh 25g of acrylic acid and dilute it with 5ml of water to obtain a mixed solution 1, dissolve 10.85g of sodium hydroxide in 25ml of water to obtain a mixed solution 2, and add the mixed solution 2 dropwise to the mixed solution 1 in an ice-water bath, control the temperature of the neutralization system to be maintained at 20-35°C, and obtain a mixed solution 3; add 0.032g of sodium dodecyl sulfate (SDS) and 0.25g of soy protein isolate powder (SPI) to 5ml of deionized water, stir at 90°C for 1h to obtain a uniform solution, cool to room temperature, adjust the pH to 10.0 with 0.1% NaOH solution, and obtain a mixed solution 4; mix the mixed solution 3 and the mixed solution 4 to obtain a mixed solution 5, add 0.025g of ethylene glycol diglycidyl ether, and heat at 45°C for 10min, then add 0.0175g of ammonium persulfate and 0.0175g of sodium bisulfite, evacuate, and introduce nitrogen to carry out free radical polymerization. The reaction was carried out at this temperature for 1 hour, then the temperature was raised to 60°C for 1 hour, and finally the temperature was raised to 80°C for 2 hours. After the reaction was completed, the product was dried at 95°C for 14 hours and crushed to obtain the degradable polymer water-absorbing resin.
[0043] Example 4
[0044] Weigh 25g of acrylic acid and dilute it with 10ml of water to obtain mixed solution 1, dissolve 11.10g of sodium hydroxide with 30ml of water to obtain mixed solution 2, add mixed solution 2 dropwise to mixed solution 1 in an ice-water bath, control the temperature of the neutralization system to be maintained at 20-35°C, and obtain mixed solution 3; add 1g of sodium dodecyl sulfate (SDS) and 2.5g of soy protein isolate powder (SPI) to 10ml of deionized water, stir at 90°C for 1h to obtain a uniform solution, cool to room temperature, adjust the pH to 6.0 with 0.1% NaOH solution, and obtain mixed solution 4; mix mixed solution 3 and mixed solution 4 to obtain mixed solution 5, add 0.0125g of poloxamer diacrylate, heat at 45°C for 10min, then add 0.0375g of ammonium persulfate and 0.0375g of sodium bisulfite, evacuate and introduce nitrogen for free radical polymerization. React at this temperature for 1h, then heat to 60°C for 1h, and finally heat to 80°C for 2h. After the reaction is completed, the product is dried at 110° C. for 8 hours and crushed to obtain the degradable polymer water-absorbent resin.
[0045] Example 5
[0046] Weigh 25g of acrylic acid and dilute it with 5ml of water to obtain mixed solution 1, dissolve 8.33g of sodium hydroxide with 30ml of water to obtain mixed solution 2, add mixed solution 2 dropwise to mixed solution 1 in an ice-water bath, control the temperature of the neutralization system to be maintained at 20-35°C, and obtain mixed solution 3; add 1.0g of sodium dodecyl sulfate (SDS) and 7.5g of soy protein isolate powder (SPI) to 15ml of deionized water, stir at 90°C for 1h to obtain a uniform solution, cool to room temperature, adjust the pH to 9.0 with 0.1% NaOH solution, and obtain mixed solution 4; mix mixed solution 3 and mixed solution 4 to obtain mixed solution 5, add 0.025g of tetraethylene glycol diacrylate, heat at 45°C for 10min, then add 0.03g of ammonium persulfate and 0.03g of sodium bisulfite, evacuate and introduce nitrogen for free radical polymerization. React at this temperature for 1h, then heat to 60°C for 1h, and finally heat to 80°C for 2h. After the reaction is completed, the product is dried at 100° C. for 12 hours and crushed to obtain the degradable polymer water-absorbent resin.
[0047] Example 6
[0048] Weigh 25g of acrylic acid and dilute it with 5ml of water to obtain mixed solution 1, dissolve 8.33g of sodium hydroxide with 25ml of water to obtain mixed solution 2, add mixed solution 2 dropwise to mixed solution 1 in an ice-water bath, control the temperature of the neutralization system to be maintained at 20-35°C, and obtain mixed solution 3; add 1.0g of sodium dodecyl sulfate (SDS) and 5.0g of soy protein isolate powder (SPI) to 15ml of deionized water, stir at 90°C for 1h to obtain a uniform solution, cool to room temperature, adjust the pH to 10.0 with 0.1% NaOH solution, and obtain mixed solution 4; mix mixed solution 3 and mixed solution 4 to obtain mixed solution 5, add 0.020g of polyethylene glycol monomethyl ether acrylate, heat at 45°C for 10min, then add 0.035g of ammonium persulfate and 0.035g of sodium bisulfite, evacuate and introduce nitrogen for free radical polymerization. React at this temperature for 1h, then heat to 60°C for 1h, and finally heat to 80°C for 2h. After the reaction is completed, the product is dried at 100° C. for 12 hours and crushed to obtain the degradable polymer water-absorbent resin.
[0049] Comparative Example 1
[0050] Weigh 25g of acrylic acid and dilute it with 5ml of water to obtain a mixed solution 1, dissolve 10.85g of sodium hydroxide in 30ml of water to obtain a mixed solution 2, add the mixed solution 2 dropwise to the mixed solution 1 in an ice-water bath, control the temperature of the neutralization system to be maintained at 20-35°C, obtain a mixed solution 3, add 0.025g of N,N'-methylenebisacrylamide to the mixed solution 3, heat it at 45°C for 10min, then add 0.05g of ammonium persulfate and 0.05g of sodium bisulfite, evacuate and introduce nitrogen for free radical polymerization. React at this temperature for 1h, then heat to 60°C for 1h, and finally heat to 80°C for 2h. After the reaction is completed, let the product dry at 100°C for 12h, and crush it to obtain the degradable polymer water-absorbing resin.
[0051] Performance Testing
[0052] The above examples and comparative examples were subjected to performance tests, including water absorption / 0.9% saline ratio, centrifugal water retention rate, and degradation rate. The specific test methods are as follows:
[0053] 1. Liquid absorption rate (g / g): Weigh a certain amount of dry resin sample, record as m1; pour all the sample into a 500ml beaker filled with distilled water (or 0.9% NaCl saline solution), let the water-absorbing resin fully swell at room temperature for 120 minutes, the resin is saturated with water, pour it onto a 100-mesh filter cloth, hang it for 10 minutes to remove excess water, and then weigh the resin weight and record it as m2. The resin water absorption rate is calculated by formula (1):
[0054]
[0055] Where: w——water absorption / 0.9% saline ratio, unit is g / g;
[0056] m1——weight of dry resin weighed, in g;
[0057] m2——The weight of the resin after being fully absorbed by the liquid, in g;
[0058] 2. Centrifugal water retention rate (g / g): Accurately weigh a certain amount of saturated swollen hydrogel and place it in a centrifuge for centrifugation (5000r / min). After 5 minutes, weigh the remaining mass and calculate the water retention R according to formula (2):
[0059]
[0060] Where: R——centrifugal water retention rate of super absorbent resin;
[0061] m1——mass of saturated gel before centrifugation;
[0062] m2 – the mass of saturated gel after centrifugation;
[0063] 3. Degradation rate (%): Weigh the dried gel (W0) and immerse it in PBS (pH=7.4) containing 1000U / ml trypsin, seal it and place it in a 37℃ incubator for incubation. The solution of the degraded sample was changed every three days. Take out the sample at the predetermined time, then wash it thoroughly with deionized water, dry it and weigh it (W t ). The degradation rate of the sample is calculated by formula (3):
[0064]
[0065] Where: Degradation——degradation rate of super absorbent resin;
[0066] W0——the mass of super absorbent resin before degradation;
[0067] W t ——The quality of super absorbent resin after degradation for a certain period of time;
[0068] The performance test results are shown in Table 1 below:
[0069] Table 1
[0070]
[0071] As can be seen from Table 1, the addition of soy protein isolate can greatly improve the degradation rate. The degradation rate of Comparative Example 1 without soy protein isolate is very low, and it can be said that almost no degradation occurs, while Examples 1 and 3 have a certain degree of degradation after adding a very small amount of soy protein isolate. In addition, compared with the water-absorbing resin obtained by using the traditional cross-linking agent N, N'-methylenebisacrylamide, the liquid absorption rate and centrifugal water retention rate obtained by the embodiment of the present invention using a cross-linking agent containing an ester bond or an ether bond are higher than those of the comparative example. Even under the premise that the amount of cross-linking agent used in the embodiment is higher than that of the comparative example, the liquid absorption performance and water retention performance of the product obtained in the embodiment are also better than those of the comparative example, which shows that the cross-linking agent selected by the present invention can expand the three-dimensional network structure of the resin, thereby improving the liquid absorption rate of the resin.
[0072] Figure 1 This is the infrared spectrum of the degradable polymer water-absorbent resin prepared in Example 1. -1 The -OH absorption peak is at 2937 cm -1 The stretching vibration absorption peak of -CH2 and -CH is 1706cm -1 The stretching vibration absorption peak of C=O in -COOH is 1579cm -1 and 1404cm -1 The antisymmetric and symmetric stretching vibration absorption peaks of C=O in -COONa are 1450cm -1 The bending vibration absorption peak of -CH2 and -CH is 511cm -1 The stretching vibration of Na-O is at 1620-1680cm -1 The C=C stretching vibration at the position disappears. The above results prove that the acrylic acid monomer has been polymerized and the residual amount is low.
[0073] Figure 2 This is a scanning electron microscope image of the degradable polymer water-absorbent resin prepared in Example 5. It can be seen that the resin surface is relatively smooth and the product after drying does not leave holes on the surface.
[0074] Figure 3 This is the mass change curve of the degradable polymer water-absorbent resin prepared in Example 5 after continuous degradation for 60 days. It can be seen that the degradation rate of the resin dropped significantly in the first three days. As time goes by, the degradation rate of the resin changes every day, and the degradation rate can reach 60.37% after 60 days, which indicates that the resin has good degradability.
[0075] The above are all preferred embodiments of the present invention, and are not intended to limit the present invention in any form. There are other variations and modifications without exceeding the technical solutions described in the claims.
Claims
1. A method for preparing a degradable polymer water-absorbent resin, characterized in that: The specific steps include: (1) Weighing acrylic acid, and diluting it with deionized water to obtain a mixed solution 1; (2) weighing sodium hydroxide particles and dissolving them in deionized water to obtain a mixed solution 2; (3) then adding the mixed solution 2 dropwise to the mixed solution 1 in an ice water bath, controlling the reaction heat during the neutralization process, to obtain a mixed solution 3; (4) adding sodium lauryl sulfate and soy protein isolate powder to deionized water, stirring to obtain a uniform solution, cooling to room temperature and adjusting the pH to obtain a mixed solution 4; (5) Mixing the mixed solution 3 and the mixed solution 4 to obtain a mixed solution 5, adding a crosslinking agent and co-heating, then adding an initiator system, evacuating the mixture and introducing nitrogen to carry out a free radical polymerization reaction; (6) After the reaction is completed, the product is dried and crushed to obtain the degradable polymer water-absorbent resin.
2. The method for preparing a degradable polymer water-absorbent resin according to claim 1, characterized in that: In the mixed solution 1 of step (1), acrylic acid accounts for 25%-40% of the total mass of the mixed solution 5; the concentration of acrylic acid in the mixed solution 1 of step (1) is 70%-85%; the mass concentration of sodium hydroxide in the mixed solution 2 of step (2) is 20%-40%.
3. The method for preparing a degradable polymer water-absorbent resin according to claim 1, characterized in that: The temperature of the reaction heat of the neutralization process in step (3) is controlled to be 20-35° C.; the degree of neutralization of the carboxyl groups in the mixed solution 3 is 60%-80%.
4. The method for preparing a degradable polymer water-absorbent resin according to claim 1, characterized in that: In step (4), the mass ratio of sodium lauryl sulfate to soy protein isolate powder is 0.125-1.20; the mass of soy protein isolate powder accounts for 0.01%-30% of the mass of acrylic acid; after cooling, the pH is adjusted to 6-10 with 0.1% NaOH solution.
5. The method for preparing a degradable polymer water-absorbent resin according to claim 1, characterized in that: The crosslinking agent in step (5) is one or more of tetraethylene glycol diacrylate, pentaerythritol dimethacrylate, poloxamer diacrylate, ethylene glycol diglycidyl ether and polyethylene glycol monomethyl ether acrylate; the crosslinking agent in the mixed solution 5 accounts for 0.1‰-1.0‰ of the mass of acrylic acid.
6. The method for preparing a degradable polymer water-absorbent resin according to claim 1, characterized in that: The initiation system in step (5) comprises an initiator and a reducing agent, wherein the initiator is one or more of potassium persulfate or ammonium persulfate; the reducing agent is one or more of sodium sulfite or sodium bisulfite; in the mixed solution 5, the initiator accounts for 0.5‰-2‰ of the mass of acrylic acid, and the reducing agent accounts for 0.5‰-2‰ of the mass of acrylic acid.
7. The method for preparing a degradable polymer water-absorbent resin according to claim 1, characterized in that: The initiation temperature of the free radical polymerization reaction in step (5) is 40-60°C, and the thermal initiation reaction time is 0.5-3h; the temperature of the free radical polymerization reaction in step (5) is 60-90°C, and the polymerization reaction time is 3-6h.
8. The method for preparing a degradable polymer water-absorbent resin according to claim 1, characterized in that: The drying temperature in step (6) is 70-110° C. and the drying time is 8-24 hours.
9. A degradable polymer water-absorbent resin prepared by the preparation method according to any one of claims 1 to 8.
10. The degradable polymer water-absorbent resin according to claim 9, characterized in that: The resin has an absorption rate of 1765 g / g for deionized water and 101 g / g for 0.9% saline, a centrifugal water retention rate of 1533 g / g, and a degradation rate of 60 days reaching 60.37%.
Citation Information
Patent Citations
Preparation method of completely biodegradable high-absorptivity resin
CN116444715A
Modified soybean protein isolate base superpower water absorbent and preparation method thereof
CN1669638A
Absorbent Soy Protein Isolate Base Hydrogels
US20090215619A1