Hydroxyl-terminated hyperbranched polyester modified hindered phenol composite material and butyl rubber damping material prepared from hydroxyl-terminated hyperbranched polyester modified hindered phenol composite material

By introducing hydroxyl-terminated hyperbranched polyester-modified hindered phenol into butyl rubber to form hydrogen bonds to improve damping performance, and adjusting the material formula, the problems of damping temperature range and glass transition temperature of butyl rubber damping materials were solved, and Provides better damping performance and wider operating temperature range.

CN118725337AInactive Publication Date: 2024-10-01AIHUA (ZHEJIANG) NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411215580.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing butyl rubber damping materials have insufficient damping temperature range, low glass transition temperature and unstable damping performance, which limits their application fields.

Method used

Using hydroxyl-terminated hyperbranched polyester-modified hindered phenol as a functional additive, it can form hydrogen bonds with polar side groups in the butyl rubber system, thereby consuming mechanical energy to improve damping performance, and adjust the glass transition temperature by adjusting the material formula. Expand the damping temperature range.

Benefits of technology

It achieves a wider damping temperature range and better peeling performance, solves the problem of low glass transition temperature of butyl rubber itself, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725337A_ABST
    Figure CN118725337A_ABST
Patent Text Reader

Abstract

The invention relates to a hydroxyl-terminated hyperbranched polyester modified hindered phenol composite material and a butyl rubber damping material prepared from the hydroxyl-terminated hyperbranched polyester modified hindered phenol composite material. The hydroxyl-terminated hyperbranched polyester modified hindered phenol composite material is introduced into a butyl rubber system as a functional additive, on one hand, hydrogen-bond interaction can be formed between the hindered phenol composite material and a polar side group in a rubber matrix, when external stress or vibration is applied, hydrogen bonds in the material are weakened or broken, and new hydrogen bonds are continuously formed, so that the service life of the material is prolonged; in the process, a large amount of energy of a system is consumed, mechanical energy is converted into internal energy, and the damping performance of the composite material is improved; on the other hand, the glass transition temperature of the rubber material can be changed, so that the effect that the optimal damping use temperature range is adjustable is achieved, and the problem that use conditions are limited due to the fact that the glass transition temperature of butyl rubber is low is solved; and meanwhile, the wider damping temperature range and the better stripping performance also conform to the diversification and functionalization development trend of the current non-vulcanized rubber damping material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of damping materials, and in particular to a hydroxyl-terminated hyperbranched polyester modified hindered phenol composite material and a butyl rubber damping material prepared using the same. Background Art

[0002] With the rapid development of China's automobile industry, the vibration and noise problems caused by vehicles moving at high speeds are becoming more and more serious. On the one hand, this problem will affect the safety and reliability of vehicle-mounted equipment, and on the other hand, it will reduce the riding experience of passengers. There are currently two commonly used solutions to this problem. One is to use a mechanical structure with a damping structure to reduce vibration, and the other is to use polymer damping materials to reduce vibration and noise.

[0003] Butyl rubber is a copolymer of isobutylene and a small amount of isoprene. Its molecular chain structure contains a large number of side methyl groups. The steric hindrance effect of these side methyl groups makes the butyl rubber molecular chain segments have large elastic hysteresis, energy dissipation and damping effects when they move. The macroscopic performance is high damping performance. In addition, butyl rubber has good air tightness, very low unsaturation, stable structure, good heat resistance and aging resistance, so it is widely used in rubber damping products. However, butyl rubber currently still has defects such as insufficient effective damping temperature range, low glass transition temperature and unstable damping performance, so its application field has certain limitations.

[0004] Hindered phenols are organic polar small molecules that are often modified and added to rubber systems as functional additives. Adding organic polar small molecules such as hindered phenols to the polymer matrix can form reversible hydrogen bonds with the polar side groups in the rubber matrix. When subjected to external stress or vibration, the hydrogen bonds in the material are weakened or broken, and new hydrogen bonds are continuously formed. This process will consume a large amount of energy in the system, convert mechanical energy into internal energy, and improve the damping performance of the composite material.

[0005] For example, in Chinese patent CN201110347024.0, a functional additive prepared by condensation reaction of dendritic organic montmorillonite and hindered phenol is added to a rubber matrix; in Chinese patent CN201510958560.2, a hindered phenol functional additive obtained by hyperbranching hindered phenol with N,N-dihydroxyethyl-3-aminopropionic acid methyl ester monomer is added to a rubber matrix; in Chinese patent CN201610195991.2, a high molecular weight hindered phenol prepared by modification is added to a rubber matrix; the above patents all adopt various measures to modify hindered phenol to obtain modified hindered phenol functional additives, which are then added to a rubber matrix to improve the damping properties of the rubber. However, the above patents can only improve the mechanical properties or damping properties of the rubber matrix, and cannot simultaneously improve the effective damping temperature range, damping properties and mechanical properties of the rubber material, especially cannot significantly change the glass transition temperature of the rubber composite material. Therefore, the development of new hindered phenol functional additives is of great practical significance for obtaining vibration and noise reduction damping materials with excellent comprehensive performance. Summary of the invention

[0006] In order to solve the above technical problems, the present application provides a terminal hydroxyl hyperbranched polyester modified hindered phenol composite material and a butyl rubber damping material prepared using the same.

[0007] The present application provides a method for preparing a hydroxyl-terminated hyperbranched polyester modified hindered phenol composite material, which is achieved by the following technical scheme: A hydroxy-terminated hyperbranched polyester grafted modified hindered phenol composite material is mainly prepared from (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride, hydroxy-terminated hyperbranched polyester grafted modified hindered phenol, and a catalyst: the catalyst is at least one of triethylamine TEA and dimethylaminopyridine DMAP; the hydroxy-terminated hyperbranched polyester grafted modified hindered phenol is prepared from polyol Bx and / or surface hydroxylated modified nano-aramid composite material as core molecules and dimethylol propionic acid DMPA as AB2 monomer; the polyol Bx is at least one of pentaerythritol, trimethylolpropane, glycerol, 2,2,6,6-tetramethylolcyclohexanol, 1,3,5-tris(2-hydroxyethyl)cyanuric acid, and 1,4-butanediol; The preparation method of (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride is as follows: under the protection of inert gas, (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acrylic acid is dissolved in chloroform, the temperature is raised to 50-70° C., thionyl chloride is slowly added dropwise to the chloroform solution, and the mixture is slowly stirred for 4-6 hours to obtain the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride; The preparation method of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material is as follows: the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride, the terminal hydroxyl hyperbranched polyester and the catalyst are stirred and reacted at 20-30° C. for 20-30 hours. After the reaction is completed, vacuum distillation is first performed, and the obtained solid residue is dissolved in dichloromethane, then extracted with NaHCO3, washed with HCl solution, and the obtained organic layer is washed with saturated brine. The obtained solution is dried and filtered with anhydrous Na2SO4, and finally vacuum dried to obtain the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material.

[0008] Furthermore, the mass ratio of the terminal hydroxyl hyperbranched polyester: (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acrylic acid: catalyst is (2-4): (20-25): (5-10).

[0009] Furthermore, the preparation method of the surface hydroxylation-modified nano-aramid composite material is as follows: S1. Preparation of nano-aramid fiber ANF; Simultaneously, preparation of isocyanate-modified halloysite nanotubes is carried out; S2. The prepared nano-aramid fiber ANF is surface-hydroxylated to obtain nano-aramid fiber ANF@OH; S3. Weigh 0.8-1.0 parts of nano-aramid fiber ANF@OH obtained in S2, 0.05-0.20 parts of isocyanate-modified halloysite nanotubes prepared in S1, 5*10-5~5*10-4 parts of organic tin catalyst, and 4-8 parts of acetone, mix them evenly, heat to 75-95°C for reaction for 0.5-1.0h, filter the product under reduced pressure, wash it with acetone and deionized water at least three times in sequence, and vacuum dry it after washing to obtain the surface hydroxylated modified nano-aramid composite material ANF@O-CO-NH@haloysite nanotubes.

[0010] Furthermore, the preparation method of the isocyanate-modified halloysite nanotubes is as follows: 10 parts of halloysite nanotubes and 50-400 parts of acetone are weighed and dispersed and mixed evenly, then 0.20-0.50 parts of isocyanate silane are added, magnetic stirring is performed at 200-400 rpm for 5-10 minutes, and then ultrasonic dispersion treatment is performed for 15-30 minutes. The obtained dispersion is filtered under nitrogen protection, and the residual acetone is removed by reduced pressure distillation, and vacuum packaging is performed to obtain isocyanate-modified halloysite nanotubes.

[0011] Furthermore, the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol with polyol Bx as the core molecule and a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composition with surface hydroxylated modified nano-aramid composite material as the core molecule.

[0012] Furthermore, the polyol Bx is a core molecule type of terminal hydroxyl hyperbranched polyester grafted modified hindered phenol, which is one of HBPE-H20, HBPE-H30, and HBPE-H40 prepared with pentaerythritol as the core molecule and dimethylolpropionic acid DMPA as the AB2 monomer; the surface hydroxylated modified nano-aramid composite material is a core molecule type of terminal hydroxyl hyperbranched polyester grafted modified hindered phenol, which is a surface hydroxylated modified nano-aramid composite material as the core molecule and dimethylolpropionic acid DMPA as the AB2 monomer.

[0013] Furthermore, the mass ratio of the polyol Bx as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol and the surface hydroxylated modified nano-aramid composite material as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is (0.5-3):1.

[0014] The present application provides a butyl rubber damping material prepared by using a hydroxyl-terminated hyperbranched polyester modified hindered phenol composite material, which is realized by the following technical scheme: A butyl rubber damping material prepared by using a terminal hydroxyl hyperbranched polyester modified hindered phenol composite material comprises the following raw materials in parts by weight: 100 parts of butyl rubber, 200-300 parts of filler, 100-150 parts of polyisobutylene, 20-40 parts of reinforcing agent, 25-40 parts of tackifier, 10-15 parts of carbon black, 5-30 parts of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material described in any one of claims 1 to 6, 2-4 parts of vulcanizing agent, 2-5 parts of dispersing agent, 4-8 parts of antioxidant and 4-10 parts of softening agent.

[0015] Furthermore, the butyl rubber is one or more of Exxon268, Xinhui 532, and Yanshan IIR1751.

[0016] Furthermore, the filler is maleimide-grafted graphene combined with at least one of talc, kaolin, titanium dioxide, montmorillonite, mica powder, calcium carbonate, barium sulfate, worm graphite, aluminum oxide, magnesium oxide, and boron nitride.

[0017] Furthermore, the polyisobutylene includes one or more of PB 680, PB1300, and PB2400.

[0018] Furthermore, the tackifier includes one or more of petroleum resin, terpene resin, phenolic resin, and epoxy resin.

[0019] Furthermore, the vulcanizing agent includes one or more of sulfur, colloidal sulfur, and sulfur monochloride.

[0020] Furthermore, the carbon black includes one or more of N330, N774, and N990.

[0021] Furthermore, the reinforcing agent includes one or more of fumed silica and precipitated silica.

[0022] Furthermore, the dispersant includes at least one of a silane coupling agent, a stearate, and a titanate coupling agent.

[0023] Furthermore, the antioxidant includes at least one of nano silicon nitride, phenolic antioxidants, and heterocyclic antioxidants.

[0024] Furthermore, the softener includes at least one of cyclohexane oil, dibutyl ester and paraffin oil.

[0025] Furthermore, the filler is composed of maleimide-grafted graphene, mica powder with a sheet diameter less than 6.5 microns, and boron nitride nanosheets with a sheet diameter less than 500 nm in a mass ratio of (5-20):(70-90):(5-10).

[0026] Furthermore, the preparation method of the maleimide-grafted graphene is as follows: first, an aminosilane coupling agent is used to modify hydroxylated graphene to obtain graphene containing amino groups on the surface; then, maleimidopropionic acid is reacted with an acyl chloride reagent to produce maleimidopropionyl chloride; the obtained maleimidopropionyl chloride and the graphene containing amino groups on the surface are dissolved in an acetone / DMF mixed solution, reacted at 60-80° C. for 3-5 hours, and after the reaction is completed, the solid obtained by vacuum filtration is placed under vacuum drying at 120-160° C. and 0.5-1.0 Pa for 4-6 hours to obtain maleimide-grafted graphene.

[0027] Furthermore, the preparation method of the butyl rubber damping material is as follows: Step 1, preparation of a hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite material and maleimide grafted graphene; Step 2: accurately measuring butyl rubber, filler, polyisobutylene, reinforcing agent, tackifier, carbon black, the hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol composite material prepared in step 1, vulcanizing agent, dispersant, antioxidant, and softener are put into an internal mixer, and mixed at 80-105° C. for 80-100 min to obtain a finished butyl rubber damping material. Furthermore, a proportion of butyl rubber and a hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite material is put into an internal mixer and mixed at 80-100° C. for 10 min; a proportion of a tackifier, carbon black, a reinforcing agent, a vulcanizing agent, a dispersant, an antioxidant, and a softener are continuously added and mixed for 20 min; half of the proportion of a filler and liquid polyisobutylene are continuously added and mixed for 20 min; the remaining half of the filler and liquid polyisobutylene are added and mixed for 30-50 min, the material is discharged, and naturally cooled to room temperature to obtain the hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite butyl damping rubber.

[0028] In summary, this application has the following advantages: 1. The present invention introduces the prepared terminal hydroxyl hyperbranched polyester grafted modified hindered phenol as a functional additive into the butyl rubber system, which can form hydrogen bonds with the polar side groups in the rubber matrix. When subjected to external stress or vibration, the hydrogen bonds in the material are weakened or broken, and new hydrogen bonds are continuously formed. This process will consume a large amount of energy in the system, convert mechanical energy into internal energy, and improve the damping performance of the composite material.

[0029] 2. By adjusting the content of terminal hydroxyl hyperbranched polyester grafted modified hindered phenol and filler, the glass transition temperature of the rubber material can be changed, and the optimal damping temperature range can be adjusted to achieve the effect of adjustable use temperature, which solves the problem of limited use conditions caused by the low glass transition temperature of butyl rubber itself, and at the same time has a wider damping temperature range and better peeling performance.

[0030] 3. The preparation process of the present invention is economical and practical, the preparation process is simple, the cost is low, no special equipment and harsh conditions are required, it is easy to achieve large-scale production, and it has extremely strong practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a synthetic route of the terminal hydroxyl hyperbranched polyester graft-modified hindered phenol composite material in the present application.

[0032] Figure 2 It is the loss factor variation curve of Examples 1-3 and Comparative Examples 1-3 in this application as a function of temperature. DETAILED DESCRIPTION

[0033] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples. Example

[0034] A hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite material is mainly prepared from (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride, hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol and a catalyst.

[0035] Preferably, the mass ratio of (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride, terminal hydroxyl hyperbranched polyester grafted modified hindered phenol, and catalyst is (2-4):(20-25):(5-10).

[0036] The catalyst is at least one of triethylamine TEA and dimethylaminopyridine DMAP.

[0037] The terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is prepared from polyol Bx and / or surface hydroxylated modified nano-aramid composite material as core molecules and dimethylol propionic acid DMPA as AB2 monomer.

[0038] Polyol B x The solvent is at least one of pentaerythritol, trimethylolpropane, glycerol, 2,2,6,6-tetramethylolcyclohexanol, 1,3,5-tris(2-hydroxyethyl)cyanuric acid and 1,4-butanediol.

[0039] Preferably, the hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol is a hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol with polyol Bx as the core molecule and a hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composition with the surface hydroxylated modified nano-aramid composite material as the core molecule.

[0040] Polyol B x The invention is one of HBPE-H20, HBPE-H30 and HBPE-H40 prepared by grafting modified hindered phenol with terminal hydroxyl group hyperbranched polyester of core molecule type and pentaerythritol as core molecule and dimethylol propionic acid DMPA as AB2 monomer.

[0041] The surface hydroxylation-modified nano-aramid composite material is a core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol, which is prepared by using the surface hydroxylation-modified nano-aramid composite material as a core molecule and dimethylol propionic acid DMPA as an AB2 monomer.

[0042] Preferably, the mass ratio of the polyol Bx as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol and the surface hydroxylated modified nano-aramid composite material as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is (0.5-3):1.

[0043] The preparation method of the surface hydroxylation-modified nano-aramid composite material is as follows: S1. Preparation of nano-aramid fiber ANF; At the same time, the preparation of isocyanate-modified halloysite nanotubes is carried out: 10 parts of halloysite nanotubes and 50-400 parts of acetone are weighed and dispersed and mixed evenly, and then 0.20-0.50 parts of isocyanate silane are added, and magnetic stirring is carried out at 200-400 rpm for 5-10 minutes, and then ultrasonic dispersion treatment is carried out for 15-30 minutes. The obtained dispersion is filtered under nitrogen protection, and the residual acetone is removed by reduced pressure distillation, and vacuum packaging is carried out to obtain isocyanate-modified halloysite nanotubes; S2. The prepared nano-aramid fiber ANF is surface-hydroxylated to obtain nano-aramid fiber ANF@OH; S3. Weigh 0.8-1.0 parts of the nano-aramid fiber ANF@OH obtained in S2, 0.05-0.20 parts of the isocyanate-modified halloysite nanotubes prepared in S1, and 5*10 -5 ~5*10 -4 After 4-8 parts of organic tin catalyst and 4-8 parts of acetone are evenly mixed, the mixture is heated to 75-95° C. and reacted for 0.5-1.0 h. The obtained product is filtered under reduced pressure and washed with acetone and deionized water at least three times in sequence. After washing, the product is vacuum dried to obtain the surface hydroxylated modified nano-aramid composite material ANF@O-CO-NH@halloysite nanotube.

[0044] The preparation method of the hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol composite material is as follows: refer to Figure 1 (1) The intermediate product - (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride is prepared as follows: under the protection of inert gas, (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acrylic acid is dissolved in chloroform, the temperature is raised to 50-70°C, thionyl chloride is slowly added dropwise to the chloroform solution, and the mixture is slowly stirred for 4-6 hours to obtain the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride; refer to Figure 1 (2) in the above. The intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride, the terminal hydroxyl hyperbranched polyester and the catalyst are stirred and reacted at 20-30°C for 20-30h. After the reaction is completed, vacuum distillation is first performed. The solid residue obtained is dissolved in dichloromethane, then extracted with NaHCO3, washed with HCl solution, and the obtained organic layer is washed with saturated brine. The obtained solution is dried and filtered with anhydrous Na2SO4, and finally vacuum dried to obtain the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material.

[0045] A butyl rubber damping material prepared by using a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material comprises the following raw materials in parts by weight: 100 parts of butyl rubber, 200-300 parts of filler, 100-150 parts of polyisobutylene, 20-40 parts of reinforcing agent, 25-40 parts of tackifier, 10-15 parts of carbon black, 5-30 parts of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material described in any one of claims 1 to 6, 2-4 parts of vulcanizing agent, 2-5 parts of dispersing agent, 4-8 parts of antioxidant and 4-10 parts of softening agent.

[0046] The butyl rubber is one or more of Exxon268, Xinhui 532 and Yanshan IIR1751.

[0047] The filler is maleimide-grafted graphene and at least one of talc, kaolin, titanium dioxide, montmorillonite, mica powder, calcium carbonate, barium sulfate, worm graphite, aluminum oxide, magnesium oxide, and boron nitride. Further, the filler is maleimide-grafted graphene, mica powder with a sheet diameter of less than 6.5 microns, and boron nitride nanosheets with a sheet diameter of less than 500 nm in a mass ratio of (5-20):(70-90):(5-10).

[0048] The preparation method of maleimide-grafted graphene is as follows: first, hydroxylated graphene is modified with an aminosilane coupling agent to obtain graphene containing amino groups on the surface; then, maleimidopropionic acid is reacted with an acyl chloride reagent to produce maleimidopropionyl chloride; the obtained maleimidopropionyl chloride and graphene containing amino groups on the surface are dissolved in an acetone / DMF mixed solution, reacted at 60-80° C. for 3-5 hours, and after the reaction is completed, the solid obtained by vacuum filtration is placed under vacuum drying at 120-160° C. and 0.5-1.0 Pa for 4-6 hours to obtain maleimide-grafted graphene.

[0049] The polyisobutylene includes one or more of PB 680, PB1300, and PB2400.

[0050] The tackifier includes one or more of petroleum resin, terpene resin, phenolic resin and epoxy resin.

[0051] The vulcanizing agent includes one or more of sulfur, colloidal sulfur, and sulfur monochloride.

[0052] The carbon black includes one or more of N330, N774 and N990.

[0053] The reinforcing agent includes one or more of fumed silica and precipitated silica.

[0054] The dispersant includes at least one of a silane coupling agent, a stearate, and a titanate coupling agent.

[0055] The antioxidant includes at least one of nano silicon nitride, phenolic antioxidant and heterocyclic antioxidant.

[0056] The softener includes at least one of naphthenic oil, dibutyl ester and paraffin oil.

[0057] A method for preparing a butyl rubber damping material prepared by using a hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol composite material comprises the following steps: Step 1, preparation of a hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite material and maleimide grafted graphene; Step 2: Put the proportion of butyl rubber and the end-hydroxyl hyperbranched polyester grafted modified hindered phenol composite material into an internal mixer and mix them at 80-100°C for 10 minutes; continue to add the proportion of tackifier, carbon black, reinforcing agent, vulcanizer, dispersant, antioxidant, and softener and continue to mix for 20 minutes; continue to add half of the proportion of filler and liquid polyisobutylene and continue to mix for 20 minutes; add the remaining half of the filler and liquid polyisobutylene and continue to mix for 30-50 minutes, discharge the material, and naturally cool it to room temperature to obtain a finished butyl rubber damping material.

[0058] Example 1: A hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite material is prepared from hydroxyl-terminated hyperbranched polyester HyPer H20, (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride, and catalyst triethylamine TEA.

[0059] The mass ratio of terminal hydroxyl hyperbranched polyester HyPer H20, (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride, and catalyst triethylamine TEA is 2:20:6.4.

[0060] A method for preparing a hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol composite material comprises the following steps: (1) Under nitrogen protection, 5.5 g of (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acrylic acid was dissolved in 50 ml of chloroform. After the temperature was raised to 50°C, 4 mL of thionyl chloride was added dropwise to the chloroform solution at a rate of 1 ml / min. The mixture was stirred at 60 rpm for 6 h. After the reaction was completed, the mixture was distilled under reduced pressure to remove unreacted thionyl chloride and excess chloroform solvent to obtain the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride; (2) Add 0.25 g of terminal hydroxyl hyperbranched polyester HyPer H20 and 50 mL of tetrahydrofuran (THF) into a three-necked flask, heat under nitrogen protection to completely dissolve the terminal hydroxyl hyperbranched polyester HyPer H20, then dissolve 1.6 g of TEA-DMAP (TEA:DMAP mass ratio 1:1) in 5 mL of tetrahydrofuran (THF) solution, add the resulting solution into the three-necked flask at a rate of 1 ml / min, heat the water bath to 50 °C and react for 1 h, then place the resulting solution in an ice bath and cool to 20 °C, then add 2.5 The intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride of 1000 g was dissolved in 10 mL of THF, and the resulting solution was dripped into a three-necked flask at a rate of 5 ml / min. The temperature was maintained at 20°C and the reaction was carried out for 20 h. After the reaction was completed, vacuum distillation was first carried out, and the solid residue was dissolved in dichloromethane, then extracted with NaHCO3, washed with HCl solution, and the organic layer was washed with saturated brine. The resulting solution was dried and filtered with anhydrous Na2SO4, and finally vacuum dried at 60°C / 4h to obtain a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material.

[0061] A butyl rubber damping material prepared by using a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material is prepared from 100 g of butyl rubber (Yanshan IIR1751), 200 g of 2000 mesh sieved mica powder, 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 6 g of the above-prepared terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, and 5 g of dibutyl ester.

[0062] A preparation method of a butyl rubber damping material prepared by using a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material is as follows: 100 g of butyl rubber (Yanshan IIR1751) and 6 g of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material prepared above are put into an internal mixer and kneaded at 80°C for 10 min; 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, and 5 g of dibutyl ester are added and kneaded for 20 min; 100 g of 2000 mesh sieved mica powder and 50 g of liquid polyisobutylene PB1300 are added and kneaded for 20 min. min; add 100g of 2000 mesh sieve mica powder and 50g of liquid polyisobutylene PB1300 and mix for 40min, discharge the material, and cool it naturally to room temperature to obtain the finished butyl rubber damping material.

[0063] The difference between Example 2 and Example 1 is that: The preparation of the hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol is as follows: (1) Under nitrogen protection, 6 g of (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acrylic acid was dissolved in 55 mL of chloroform. After the temperature was raised to 60°C, 5 mL of thionyl chloride was added dropwise to the chloroform solution at a rate of 1 ml / min. After stirring for 5 h, the mixture was distilled under reduced pressure to remove unreacted thionyl chloride and excess chloroform solvent to obtain the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride; (2) Add 0.3 g of terminal hydroxyl hyperbranched polyester HyPer H20 and 55 mL of tetrahydrofuran (THF) into a three-necked flask, heat under nitrogen protection to completely dissolve the terminal hydroxyl hyperbranched polyester HyPer H20, then dissolve 1.8 g of TEA-DMAP (TEA:DMAP mass ratio 1:1) in 5 mL of tetrahydrofuran (THF) solution, add the solution into the three-necked flask at a rate of 1 ml / min, react at 50 °C for 1 h, then place the resulting solution in an ice bath to cool to 25 °C, and then heat for 3 hours. The intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride of g was dissolved in 10mL of tetrahydrofuran (THF), and then dripped into a three-necked flask at a rate of 5ml / min and maintained at 25°C for reaction for 25h. After the reaction, it was firstly distilled under reduced pressure, and the solid residue was dissolved in dichloromethane, then extracted with NaHCO3, washed with HCl solution, and the organic layer was washed with saturated brine. The solution was dried and filtered with anhydrous Na2SO4, and finally vacuum dried at 60°C / 4h to obtain a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material.

[0064] A butyl rubber damping material prepared by using a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material is prepared from 100 g of butyl rubber (Yanshan IIR1751), 250 g of 2000 mesh sieved mica powder, 125 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 18 g of the above-prepared terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material, 3 g of sulfur, 4 g of KH550, 6 g of antioxidant 2246, and 6 g of dibutyl ester.

[0065] A preparation method of a butyl rubber damping material prepared by using a hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite material is as follows: 100 g of butyl rubber (Yanshan IIR1751) and 18 g of the prepared hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite material are put into an internal mixer and kneaded at 90° C. for 10 min; 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 3 g of sulfur, 4 g of KH550, 6 g of antioxidant 2246, and 6 g of dibutyl ester are added and kneaded for 20 min; 125 g of 2000 mesh sieved mica powder and 62.5 g of liquid polyisobutylene PB1300 are added and kneaded for 20 min. min; add 125g of 2000 mesh sieve mica powder and 62.5g of liquid polyisobutylene PB1300 and mix for 40min, discharge the material, and cool it naturally to room temperature to obtain the finished butyl rubber damping material.

[0066] The difference between Example 3 and Example 1 is that the preparation of the hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol is as follows: (1) Under nitrogen protection, 6.5 g of (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acrylic acid was dissolved in 60 mL of chloroform. After the temperature was raised to 70°C, 6 mL of thionyl chloride was added dropwise to the chloroform solution at a rate of 1 ml / min. The mixture was stirred for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure to remove unreacted thionyl chloride and excess chloroform solvent to obtain the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride; (2) Add 0.35 g of terminal hydroxyl hyperbranched polyester HyPer H20 and 60 mL of tetrahydrofuran (THF) into a three-necked flask, heat under nitrogen protection to completely dissolve the terminal hydroxyl hyperbranched polyester HyPer H20, then dissolve 2 g of TEA-DMAP (TEA:DMAP mass ratio 1:1) in 5 mL of tetrahydrofuran (THF) solution, add the resulting solution into the three-necked flask at a rate of 1 ml / min, heat to 50 °C in a water bath and react for 1 h, then place the resulting solution in an ice bath and cool to 30 °C, then dissolve 3.5 g of the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride in 10 mL of tetrahydrofuran (THF), the resulting solution was dripped into a three-necked flask at a rate of 5 ml / min, and the temperature was maintained at 30°C for 30 hours. After the reaction was completed, vacuum distillation was first performed, and the solid residue was dissolved in dichloromethane, then extracted with NaHCO3, washed with HCl solution, and the organic layer was washed with saturated brine. The resulting solution was dried and filtered with anhydrous Na2SO4, and finally vacuum dried at 60°C / 4h to obtain a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material.

[0067] A butyl rubber damping material prepared by using a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material is prepared from 100 g of butyl rubber (Yanshan IIR1751), 300 g of 2000 mesh sieved mica powder, 150 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 30 g of the above-prepared terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material, 4 g of sulfur, 6 g of KH550, 8 g of antioxidant 2246, and 8 g of dibutyl ester.

[0068] A preparation method of a butyl rubber damping material prepared by using a terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material is as follows: 100 g of butyl rubber (Yanshan IIR1751) and 30 g of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material prepared above are put into an internal mixer and kneaded at 100°C for 10 min; 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 4 g of sulfur, 6 g of KH550, 8 g of antioxidant 2246, and 8 g of dibutyl ester are added and kneaded for 20 min; 150 g of 2000 mesh sieved mica powder and 75 g of liquid polyisobutylene PB1300 are added and kneaded for 20 min. min; add 150g of 2000 mesh sieve mica powder and 75g of liquid polyisobutylene PB1300 and mix for 40min, discharge the material, and cool it naturally to room temperature to obtain the finished butyl rubber damping material.

[0069] The difference between Example 4 and Example 1 is that the butyl rubber damping material prepared by using the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material is composed of 100 g of Yanshan IIR1751 butyl rubber, 10 g of maleimide grafted graphene, 180 g of 2000 mesh sieved mica powder, 10 g of boron nitride nanosheets (average thickness: <100 nm, sheet diameter: 1-3 μm, specific surface area: 30 m 2 / g, particle form: flake; CAS: 10043-11-5, brand Kemik), 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 6 g of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material prepared in Example 1, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, 2 g of nano silicon nitride (flake high-purity nano silicon nitride powder with an average particle size of 50-200 nm, brand Wenlun Metal), and 5 g of dibutyl ester.

[0070] The preparation method of maleimide grafted graphene is as follows: S1. First, aminosilane coupling agent is used to modify hydroxylated graphene to obtain graphene with amino groups on the surface: 1g of hydroxylated graphene (Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, hydroxylated graphene TNRGOH, thickness: 0.55~3.74nm; diameter: 0.5-3μm; number of layers: <10 layers; oxygen content: >10wt%) and 50mL of toluene are placed in a 250mL beaker, and transferred to an ultrasonic disperser for 1.0h ultrasonic dispersion treatment, with an ultrasonic dispersion frequency of 40kHz and a power of 800W, and then 0.3g of γ-aminopropyltriethoxysilane is added, and the temperature is controlled at 30°C in a water bath to react for 6h. After the reaction is completed, vacuum filtration is performed to obtain a solid powder, and the obtained solid powder is placed at 80°C and vacuum dried for 12h to obtain graphene with amino groups on the surface; S2. Maleimidopropionic acid is reacted with an acyl chloride reagent to obtain maleimidopropionyl chloride: 3.6 g of maleimidopropionic acid (molecular weight 169.135, CAS: 7423-55-4) is added dropwise with 1.5 g of thionyl chloride in 100 mL of N,N-dimethylformamide (DMF), and the mixture is reacted at 30° C. in a water bath for 8 h to obtain a mixed solution containing maleimidopropionyl chloride; S3. Weigh 25 mL of the mixed solution containing maleimidopropionyl chloride prepared in S2 and 1 g of graphene with amino groups on the surface prepared in S1, dissolve them in 25 mL of acetone / DMF mixed solution (acetone / DMF volume is 1:1), react at 65°C for 5 h, and after the reaction is completed, vacuum filter the obtained solid and place it under vacuum drying at 125°C and 0.5 Pa for 6 h to obtain maleimide-grafted graphene.

[0071] The difference between Example 5 and Example 4 is that the butyl rubber damping material prepared by using the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material is composed of 100 g of Yanshan IIR1751 butyl rubber, 20 g of maleimide grafted graphene, 165 g of 2000 mesh sieved mica powder, 15 g of boron nitride nanosheets (average thickness: <100 nm, sheet diameter: 1-3 μm, specific surface area: 30 m 2 / g, particle form: flake; CAS: 10043-11-5, brand Kemik), 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 6 g of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material prepared in Example 1, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, 2 g of nano silicon nitride (flake high-purity nano silicon nitride powder with an average particle size of 50-200 nm, brand Wenlun Metal), and 5 g of dibutyl ester.

[0072] The difference between Example 6 and Example 4 is that the butyl rubber damping material prepared by using the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material is composed of 100 g of Yanshan IIR1751 butyl rubber, 40 g of maleimide grafted graphene, 140 g of 2000 mesh sieved mica powder, 20 g of boron nitride nanosheets (average thickness: <100 nm, sheet diameter: 1-3 μm, specific surface area: 30 m 2 / g, particle form: flake; CAS: 10043-11-5, brand Kemik), 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 6 g of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material prepared in Example 1, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, 2 g of nano silicon nitride (flake high-purity nano silicon nitride powder with an average particle size of 50-200 nm, brand Wenlun Metal), and 5 g of dibutyl ester.

[0073] The difference between Example 7 and Example 4 is that the butyl rubber damping material prepared by using the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material is composed of 100 g of Yanshan IIR1751 butyl rubber, 45 g of maleimide grafted graphene, 130 g of 2000 mesh sieved mica powder, 25 g of boron nitride nanosheets (average thickness: <100 nm, sheet diameter: 1-3 μm, specific surface area: 30 m 2 / g, particle form: flake; CAS: 10043-11-5, brand Kemik), 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 6 g of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material prepared in Example 1, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, 2 g of nano silicon nitride (flake high-purity nano silicon nitride powder with an average particle size of 50-200 nm, brand Wenlun Metal), and 5 g of dibutyl ester.

[0074] The difference between Example 8 and Example 4 is that the butyl rubber damping material prepared by using the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material is composed of 100 g of Yanshan IIR1751 butyl rubber, 5 g of maleimide grafted graphene, 190 g of 2000 mesh sieved mica powder, 5 g of boron nitride nanosheets (average thickness: <100 nm, sheet diameter: 1-3 μm, specific surface area: 30 m 2 / g, particle form: flake; CAS: 10043-11-5, brand Kemik), 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 6 g of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material prepared in Example 1, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, 2 g of nano silicon nitride (flake high-purity nano silicon nitride powder with an average particle size of 50-200 nm, brand Wenlun Metal), and 5 g of dibutyl ester.

[0075] The difference between Example 9 and Example 4 is that the butyl rubber damping material prepared by using the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material is made of 100 g of Yanshan IIR1751 butyl rubber, 50 g of maleimide grafted graphene, 150 g of 2000 mesh sieved mica powder, 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 6 g of the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material prepared in Example 1, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, 2 g of nano silicon nitride (flaky high-purity nano silicon nitride powder with an average particle size of 50-200 nm, brand Wenlun Metal), and 5 g of dibutyl ester.

[0076] The difference between Example 10 and Example 4 is that the butyl rubber damping material prepared by using the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material is composed of 100 g of Yanshan IIR1751 butyl rubber, 50 g of boron nitride nanosheets (average thickness: <100 nm, sheet diameter: 1-3 μm, specific surface area: 30 m 2 / g, particle form: flake; CAS: 10043-11-5, brand Kemik), 150 g of 2000 mesh sieved mica powder, 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 6 g of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material prepared in Example 1, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, 2 g of nano silicon nitride (flaky high-purity nano silicon nitride powder with an average particle size of 50-200 nm, brand Wenlun Metal), and 5 g of dibutyl ester.

[0077] The difference between Example 11 and Example 1 is that the hydroxyl-terminated hyperbranched polyester HyPer H20 is replaced by the hydroxyl-terminated hyperbranched polyester Boltorn HBPE-H20 (each molecule has 16 terminal hydroxyl groups, Mn = 1747 g / mol, Swedish Perstorp AB, Mw / Mn = 1.3, Tg = 25°C). Boltorn HBPE-H20 is a second-generation hyperbranched macromolecular polymer obtained by esterification reaction of pentaerythritol as the core molecule with dimethylol propionic acid.

[0078] The difference between Example 12 and Example 1 is that the terminal hydroxyl hyperbranched polyester graft modified hindered phenol is a surface hydroxylated modified nano-aramid composite material as a core molecule type terminal hydroxyl hyperbranched polyester graft modified hindered phenol. The surface hydroxylated modified nano-aramid composite material as a core molecule type terminal hydroxyl hyperbranched polyester graft modified hindered phenol is made of a surface hydroxylated modified nano-aramid composite material as a core molecule and dimethylol propionic acid DMPA as an AB2 monomer.

[0079] The preparation method of the surface hydroxylation-modified nano-aramid composite material is as follows: S1. Preparation of nano-aramid fiber ANF: 1028g of nitrogen methyl pyrrolidone, 54.1g of calcium chloride, and 5.4g of polyvinyl pyrrolidone were added in sequence into a 3L custom-made three-necked flask filled with nitrogen, and stirred at 70°C for 60min until all the solid substances were dissolved; sodium chloride aqueous solution and ice cubes were used as heat exchange media to cool the system to below 4°C, and then 27.04g of p-phenylenediamine was added and stirred at 400rpm until all the solid substances were dissolved to obtain a pink transparent solution; then 54.31g of terephthaloyl was added. Chlorine, adjust the speed to 1500rpm, stir for 1min, add 39.71g of pyridine, react for 90min, and perform vacuum distillation after the reaction. The solid obtained is dispersed in dimethyl sulfoxide (DMSO) to obtain an ANF / dimethyl sulfoxide DMSO solution with a solid content of 0.5wt%. The 0.5wt% ANF / dimethyl sulfoxide DMSO solution is vacuum filtered to obtain nano-aramid fiber ANF solid material. The obtained solid powder is placed at 80°C and vacuum dried for 12h to obtain the finished nano-aramid fiber ANF. At the same time, the preparation of isocyanate-modified halloysite nanotubes was carried out: 10 g of halloysite nanotubes and 90 mL of acetone were weighed and dispersed and mixed evenly, and then 0.4 g of 3-isocyanatepropyltriethoxysilane was added, and magnetic stirring was carried out at 240 rpm for 10 min, and then ultrasonic dispersion treatment was carried out for 15 min, the ultrasonic dispersion frequency was 40 kHz, the power was 800 W, and the temperature was controlled at 30° C. in a water bath to react for 6 h. After the reaction was completed, the obtained dispersion was vacuum filtered under nitrogen protection, the obtained solid powder was washed three times with acetone, and then the residual acetone was removed by reduced pressure distillation, and then vacuum dried at 60° C. for 12 h to obtain isocyanate-modified halloysite nanotubes, and vacuum packaged; S2. The prepared nano-aramid fiber ANF was subjected to surface hydroxylation modification to obtain nano-aramid fiber ANF@OH: 1 mol of DMSO and 1 mol of NaH were mixed to prepare DMSO sodium salt, 10 g of DMSO sodium salt and 1 g of the nano-aramid fiber ANF prepared in S1 were heated to 60 °C for 0.5 h, and Na + Introduced into the surface of nano-aramid fiber ANF, vacuum filtration can be used to obtain the surface introduced Na + Modified nano-aramid fiber ANF; the surface of the obtained fiber is introduced with Na + The modified nano-aramid fiber ANF was washed three times with dimethyl sulfoxide to remove the residual DMSO sodium salt on the surface, and then dissolved in 49g of dimethyl sulfoxide, first magnetically stirred at 200rpm for 0.5h, and then transferred to an ultrasonic disperser for 45min of ultrasonic dispersion treatment, with an ultrasonic dispersion frequency of 40kHz and a power of 800W, and then 0.25g of chloropropyltrimethoxysilane ClCH2CH2CH2Si(-OCH3)3 was added and fully reacted to obtain the nano-aramid fiber ANF@CH2CH2CH2Si(-OCH3)3, and hydrolyzed to obtain the nano-aramid fiber ANF@CH2CH2CH2Si(-OH)3; S3. Weigh 10 g of nano-aramid fiber ANF@ CH2CH2CH2Si(-OH)3 obtained in S2, 2 g of isocyanate-modified halloysite nanotubes prepared in S1, 4*10 -3 After g of stannous octoate catalyst and 78 g of acetone were mixed evenly, the mixture was heated to 85 °C for reaction for 40 min, and the obtained product was filtered under reduced pressure and washed three times with acetone and deionized water in sequence. After washing, the product was vacuum dried at 80 °C for 12 h to obtain the surface hydroxylated modified nano-aramid composite material ANF@O-CO-NH@halloysite nanotubes.

[0080] The preparation method of the surface hydroxylation-modified nano-aramid composite material which is a core-type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is as follows: (1) Under nitrogen protection, 5.5 g of (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acrylic acid is dissolved in 50 ml of chloroform, and after the temperature is raised to 50°C, 4 mL of dichlorothionyl is added dropwise to the chloroform solution at a rate of 1 drop / 5s, and the mixture is stirred at 60 rpm for 6 hours. After the reaction is completed, the mixture is distilled under reduced pressure to remove unreacted dichlorothionyl and excess chloroform solvent to obtain the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride; (2) Preparation of surface hydroxylation-modified nano-aramid composite material as core-type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol: 1 g of surface hydroxylation-modified nano-aramid composite material ANF@O-CO-NH@halloysite nanotubes, 12 g of 2,2-dihydroxymethylpropionic acid, and 0.1 g of p-toluenesulfonic acid were placed in a flask, and mechanical stirring was continued under a nitrogen atmosphere. The oil bath was heated to 140°C. When the reactants in the three-necked flask melted, the melt was reacted under an inert atmosphere at normal pressure for 20 min, and vacuum distilled for 20 min to completely remove the water. The product A is completely evaporated, and N,N-dimethylformamide (DMF) is added to continue the reaction at 140° C. until the reactants are completely dispersed in DMF to obtain product B, and product B is centrifuged at 8000 rpm / 5 min, and the supernatant is poured out to obtain product C. Product C is attached to the wall of the test tube, and chloroform is added to product C. The solid product D obtained by removing unreacted monomers and DMF reagents is obtained, and the chloroform is removed in vacuum to obtain a surface hydroxylated modified nano-aramid composite material that is a core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol; (3) Add 0.25 g of the surface hydroxylated modified nano-aramid composite material prepared in (2) as the core molecule type of terminal hydroxyl hyperbranched polyester grafted modified hindered phenol and 50 mL of tetrahydrofuran (THF) into a three-necked flask, heat under nitrogen protection to completely dissolve the terminal hydroxyl hyperbranched polyester HyPer H20, then dissolve 1.6 g of triethylamine (TEA) in 30 mL of tetrahydrofuran (THF) solution, add the resulting solution into the three-necked flask at a rate of 1 drop / 5 s, heat the water bath to 50 °C and react for 1 h, then place the resulting solution in an ice bath and cool to 20 °C, then add 2.5 The intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride of 1 g was dissolved in 30 mL of THF, and the resulting solution was dripped into a three-necked flask at a rate of 1 drop / 5 s. The temperature was maintained at 20°C and the reaction was carried out for 20 h. After the reaction was completed, vacuum distillation was first carried out, and the solid residue was dissolved in dichloromethane, then extracted with NaHCO3, washed with HCl solution, and the organic layer was washed with saturated brine. The resulting solution was dried and filtered with anhydrous Na2SO4, and finally vacuum dried to obtain the finished product of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material.

[0081] The difference between Example 13 and Example 12 is that the terminal hydroxyl hyperbranched polyester HyPer H20 is replaced by Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol. The mass ratio of Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol is 1:2.

[0082] The difference between Example 14 and Example 12 is that the terminal hydroxyl hyperbranched polyester HyPer H20 is replaced by Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol. The mass ratio of Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol is 1:1.

[0083] The difference between Example 15 and Example 12 is that the terminal hydroxyl hyperbranched polyester HyPer H20 is replaced by Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol. The mass ratio of Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol is 2:1.

[0084] The difference between Example 16 and Example 12 is that the terminal hydroxyl hyperbranched polyester HyPer H20 is replaced by Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol. The mass ratio of Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol is 3:1.

[0085] The difference between Example 17 and Example 12 is that the terminal hydroxyl hyperbranched polyester HyPer H20 is replaced by Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol. The mass ratio of Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol is 4:1.

[0086] The difference between Example 18 and Example 12 is that the terminal hydroxyl hyperbranched polyester HyPer H20 is replaced by Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol. The mass ratio of Boltorn HBPE-H20 and the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester graft-modified hindered phenol is 1:3.

[0087] The difference between Example 19 and Example 14 is that the butyl rubber damping material prepared by using the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material is composed of 100 g of Yanshan IIR1751 butyl rubber, 20 g of maleimide grafted graphene, 165 g of 2000 mesh sieved mica powder, 15 g of boron nitride nanosheets (average thickness: <100 nm, sheet diameter: 1-3 μm, specific surface area: 30 m 2 / g, particle form: flake; CAS: 10043-11-5, brand Kemik), 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 3 g of terminal hydroxyl hyperbranched polyester Boltorn HBPE-H20, 3 g of the surface hydroxylated modified nano-aramid composite material prepared in Example 12 is a core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, 2 g of nano-silicon nitride (flaky high-purity nano-silicon nitride powder with an average particle size of 50-200 nm, brand Wenlun Metal), and 5 g of dibutyl ester.

[0088] The difference between Comparative Example 1 and Example 1 is that no hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol is added.

[0089] The butyl rubber damping material is made of 100 g of butyl rubber (Yanshan IIR1751), 200 g of mica powder, 100 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 2.5 g of sulfur, 3 g of KH550, 6 g of antioxidant 2246, and 5 g of dibutyl ester.

[0090] The difference between Comparative Example 2 and Example 1 is that no hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol is added.

[0091] The butyl rubber damping material is made of 100 g of butyl rubber (Yanshan IIR1751), 250 g of mica powder, 125 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 3 g of sulfur, 4 g of KH550, 6 g of antioxidant 2246, and 6 g of dibutyl ester.

[0092] The difference between Comparative Example 3 and Example 1 is that no hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol is added.

[0093] The butyl rubber damping material is made of 100 g of butyl rubber (Yanshan IIR1751), 300 g of mica powder, 150 g of PB1300, 30 g of terpene resin, 30 g of fumed silica, 10 g of N330 carbon black, 4 g of sulfur, 6 g of KH550, 8 g of antioxidant 2246, and 8 g of dibutyl ester.

[0094] Performance testing: 1. The method reported in "Hyperbranched Polymers" (Tan Huimin, Luo Yunjun. Chemical Industry Press. 2005) was used to test the branching degree, molecular weight, and molecular weight distribution index of the hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol.

[0095] Calculation of the degree of branching: According to Frechet's definition of the average degree of branching (DB), the average degree of branching of the hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol is calculated according to formula (1): DB = (D + T) / (D + T + L) (1); where D, L and T are the molar fractions of the repeating units of the dendritic structure, linear structure and terminal structure, respectively, which can be expressed by the peak area of ​​the relevant spectrum. When DB = 1, it is a dendritic molecule; when DB < 1, it is a hyperbranched polymer.

[0096] Molecular weight is determined based on the gel permeation chromatography (GPC) method. By measuring the elution time of the polymer in the gel column, combined with the elution time of a known standard, the molecular weight of the polymer can be calculated.

[0097] The molecular weight distribution index is measured based on the gel permeation chromatography (GPC) method, and the molecular weight distribution curve obtained provides the molecular weight and distribution information of the polymer.

[0098] The test data on the branching degree, molecular weight and molecular weight distribution index of the prepared hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol are shown in Table 1.

[0099] 2. Glass transition temperature of rubber: tested by DMA-242E dynamic thermomechanical analyzer produced by NETZSCH, Germany. Damping performance test: specimen thickness is 1.0 mm, test conditions: frequency 10 Hz, temperature rise from -105°C to 120°C, temperature rise frequency 3°C / min, deformation mode single cantilever beam.

[0100] 3. Mechanical properties test of rubber: GB / T 2790-1995 is used to test the mechanical properties of rubber.

[0101] 4. High-frequency damping performance test: According to ASTME 756, the high-frequency damping performance of the sample is tested on the VBT-Oberst vibration beam turntable test system. The sample is prepared according to the preparation method of the finished hot melt adhesive plugging cover in Examples 1-40 and Comparative Examples 1-18. The total thickness of the sample is 2.0 mm, the width is 12.5 mm, and the length is 215 mm. Specifically, the release paper of the sample cut to size is torn off and attached to a steel bar with a thickness of 1 mm / width of 12.5 mm / length of 241 mm. The steel bar to be tested with the sample attached is vertically clamped at one end, and the steel bar is excited to vibrate at an excitation frequency of 1 to 1000 Hz by a non-contact electromagnetic exciter located near the free end; the response of the steel bar to various frequency excitations is measured by a properly positioned sensor, and the vibration amplitude of the test sample is detected. The damping performance is represented by the loss coefficient. When the loss coefficient of the sample under 1000 Hz high-frequency excitation is not less than 0.1, it is considered to meet the application requirements, and the interval temperature of tanδ≥0.1 is recorded.

[0102] Table 1: Branching degree, molecular weight, and molecular weight distribution index of hindered phenol grafted with terminal hydroxyl hyperbranched polyester.

[0103]

[0104] Table 2: Test parameters of butyl rubber damping materials in Example 1 and Examples 4-19

[0105] Combined with Examples 1-3 and Comparative Examples 1-3 and Tables 1-2 and Figure 2 It can be seen that the butyl rubber damping material prepared by introducing the terminal hydroxyl hyperbranched polyester modified hindered phenol composite material into the butyl rubber system as a functional additive has good damping performance; and the terminal hydroxyl hyperbranched polyester modified hindered phenol composite material can change the glass transition temperature of the butyl rubber damping material, thereby achieving the effect of adjustable temperature range for optimal damping, which solves the problem of limited use conditions caused by the low glass transition temperature of butyl rubber itself. At the same time, the wider damping temperature range and better peeling performance are also in line with the current development trend of diversification and functionalization of non-vulcanized rubber damping materials.

[0106] Combining Example 1 and Example 4-10 and Table 2, it can be seen that the butyl rubber damping material of Example 1 in which the filler is only 2000 mesh sieved mica powder is compared with the butyl rubber damping material of Example 4-10 prepared by forming a composite filler with 2000 mesh sieved mica powder and maleimide grafted graphene and / or boron nitride nanosheets. The effective damping temperature range (10Hz, tanδ>0.3) of Example 4-10 is wider, and the high-frequency damping performance (temperature range of tanδ≥0.1) of Example 4-10 is also relatively wide, that is, the butyl rubber damping material prepared by the composite filler has better damping performance.

[0107] It can be seen from Example 1 and Example 4-10 and Table 2 that the damping performance of the butyl rubber damping material prepared by compounding maleimide-grafted graphene, mica powder sieved out of 2000 mesh, and boron nitride nanosheets is relatively good. From the perspective of production economic cost, maleimide-grafted graphene, mica powder sieved out of 2000 mesh, and boron nitride nanosheets are relatively good in a mass ratio of (5-20): (70-90): (5-10). Preferably, maleimide-grafted graphene, mica powder sieved out of 2000 mesh, and boron nitride nanosheets are composed of a mass ratio of 20:165:15, and the prepared butyl rubber damping material has good comprehensive performance and good economy.

[0108] From Example 1 and Examples 12-18 and Table 2, it can be seen that the effective damping temperature range (10 Hz, tanδ>0.3) and high-frequency damping performance (temperature range of tanδ≥0.1) of the butyl rubber damping material prepared by using the surface hydroxylated modified nano-aramid composite material provided in Example 12 as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol are uniformly broadened, thereby improving the damping performance of the butyl rubber damping material.

[0109] Combining Example 1 and Example 12-18 and Table 2, it can be seen that, considering the actual production cost, although the damping performance of the butyl rubber damping material prepared by the pure surface hydroxylated modified nano-aramid composite material as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is more excellent, the overall production cost is relatively high. In order to achieve the purpose of industrial production, the butyl rubber damping material prepared by the hydroxyl hyperbranched polyester grafted modified hindered phenol with the mass ratio of polyol Bx as the core molecule type and the surface hydroxylated modified nano-aramid composite material as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is (0.5-3): 1, and the damping performance of the prepared butyl rubber damping material is relatively good and the production economy is good.

[0110] In combination with Example 1, Examples 4-10, Examples 12-19 and Table 2, it can be seen that the butyl rubber damping material prepared by using the optimal filler formula in Example 5 (maleimide-grafted graphene, 2000 mesh sieved mica powder, and boron nitride nanosheets in a mass ratio of 20:165:15) in combination with the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composition formula in Example 14 (pentaerythritol as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol, surface hydroxylated modified nano-aramid composite material as the core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol The mass ratio is 1:1), the damping performance of the prepared butyl rubber damping material is relatively excellent and the production economy is good.

[0111] Combining Example 1 and Examples 12-19 and Table 2, it can be seen that the tear strength of the butyl rubber damping material in Examples 12-19 is improved by 42.37%, 38.81%, 34.72%, 29.35%, 24.82%, 18.39%, 40.37% and 49.51% respectively relative to the butyl rubber damping material in Example 1; the tensile strength of the butyl rubber damping material in Examples 12-19 is improved by 53.14%, 46.72%, 41.05%, 34.79%, 30.17%, 24.02%, 50.09% and 58.54% respectively relative to the butyl rubber damping material in Example 1. It can be seen that the surface hydroxylated modified nano-aramid composite material is a core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol which can not only improve the damping performance of the butyl rubber damping material, but also effectively improve the mechanical strength of the butyl rubber damping material.

[0112] The softening point of the butyl rubber damping material prepared in Example 5, Example 14, and Example 19 is improved relative to the softening point of the butyl rubber damping material prepared in Example 1, which improves the heat resistance stability of the butyl rubber damping material.

[0113] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A hydroxy-terminated hyperbranched polyester grafted modified hindered phenol composite material, characterized in that: The invention is mainly prepared from (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride, a terminal hydroxy hyperbranched polyester grafted modified hindered phenol, and a catalyst. The catalyst is at least one of triethylamine TEA and dimethylaminopyridine DMAP. The terminal hydroxy hyperbranched polyester grafted modified hindered phenol is a polyol B. x and / or surface hydroxylated modified nano-aramid composite material as core molecule, dimethylol propionic acid DMPA as AB2 monomer; the polyol B x At least one of pentaerythritol, trihydroxymethylpropane, glycerol, 2,2,6,6-tetrahydroxymethylcyclohexanol, 1,3,5-tris(2-hydroxyethyl)cyanuric acid, and 1,4-butanediol; The preparation method of (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride is as follows: under the protection of inert gas, (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acrylic acid is dissolved in chloroform, the temperature is raised to 50-70° C., thionyl chloride is slowly added dropwise to the chloroform solution, and the mixture is slowly stirred for 4-6 hours to obtain the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride; The preparation method of the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material is as follows: the intermediate product (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl) acryloyl chloride, the terminal hydroxyl hyperbranched polyester and the catalyst are stirred and reacted at 20-30° C. for 20-30 hours. After the reaction is completed, vacuum distillation is first performed, and the obtained solid residue is dissolved in dichloromethane, then extracted with NaHCO3, washed with HCl solution, and the obtained organic layer is washed with saturated brine. The obtained solution is dried and filtered with anhydrous Na2SO4, and finally vacuum dried to obtain the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composite material.

2. The hydroxy-terminated hyperbranched polyester graft-modified hindered phenol composite material according to claim 1, characterized in that: The mass ratio of the (E)-3-(3,5-di-tert-butyl-4-hydroxyphenyl)acryloyl chloride, the terminal hydroxyl hyperbranched polyester grafted modified hindered phenol, and the catalyst is (2-4):(20-25):(5-10).

3. The hydroxy-terminated hyperbranched polyester graft-modified hindered phenol composite material according to claim 1, characterized in that: The preparation method of the surface hydroxylation-modified nano-aramid composite material: S1. Preparation of nano-aramid fiber ANF; The preparation of isocyanate-modified halloysite nanotubes is also carried out; S2. The prepared nano-aramid fiber ANF is surface-hydroxylated to obtain nano-aramid fiber ANF@OH; S3. Weigh 0.8-1.0 parts of the nano-aramid fiber ANF@OH obtained in S2, 0.05-0.20 parts of the isocyanate-modified halloysite nanotubes prepared in S1, and 5*10 -5 ~5*10 -4 After 4-8 parts of organic tin catalyst and 4-8 parts of acetone are evenly mixed, the mixture is heated to 75-95° C. and reacted for 0.5-1.0 h. The obtained product is filtered under reduced pressure and washed with acetone and deionized water at least three times in sequence. After washing, the product is vacuum dried to obtain the surface hydroxylated modified nano-aramid composite material ANF@O-CO-NH@halloysite nanotube.

4. The hydroxy-terminated hyperbranched polyester graft-modified hindered phenol composite material according to claim 3, characterized in that: The preparation method of the isocyanate-modified halloysite nanotubes is as follows: 10 parts of halloysite nanotubes and 50-400 parts of acetone are weighed and dispersed and mixed evenly, and then 0.20-0.50 parts of isocyanate silane are added, and magnetic stirring is performed at 200-400 rpm for 5-10 minutes, and then ultrasonic dispersion treatment is performed for 15-30 minutes. The obtained dispersion is filtered under nitrogen protection, and the residual acetone is removed by reduced pressure distillation, and vacuum packaging is performed to obtain the isocyanate-modified halloysite nanotubes.

5. The hydroxy-terminated hyperbranched polyester graft-modified hindered phenol composite material according to claim 3, characterized in that: The terminal hydroxy hyperbranched polyester graft modified hindered phenol is polyol B x The core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol and the surface hydroxylated modified nano-aramid composite material are core molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol composition; the polyol B x The core molecule type of terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is one of HBPE-H20, HBPE-H30 and HBPE-H40 prepared with pentaerythritol as the core molecule and dimethylol propionic acid DMPA as the AB2 monomer; the surface hydroxylated modified nano-aramid composite material is a core molecule type of terminal hydroxyl hyperbranched polyester grafted modified hindered phenol, which is a surface hydroxylated modified nano-aramid composite material as the core molecule and dimethylol propionic acid DMPA as the AB2 monomer.

6. The hydroxy-terminated hyperbranched polyester graft-modified hindered phenol composite material according to claim 5, characterized in that: The polyol B x The mass ratio of the core-molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol and the surface hydroxylation modified nano-aramid composite material as the core-molecule type terminal hydroxyl hyperbranched polyester grafted modified hindered phenol is (0.5-3):

1.

7. A butyl rubber damping material prepared by using the hydroxy-terminated hyperbranched polyester graft-modified hindered phenol composite material according to any one of claims 1 to 6, characterized in that: The butyl rubber damping material comprises the following raw materials in parts by weight: 100 parts of butyl rubber, 200-300 parts of filler, 100-150 parts of polyisobutylene, 20-40 parts of reinforcing agent, 25-40 parts of tackifier, 10-15 parts of carbon black, 5-30 parts of the hydroxy-terminated hyperbranched polyester graft-modified hindered phenol composite material according to any one of claims 1-6, 2-4 parts of vulcanizing agent, 2-5 parts of dispersant, 4-8 parts of antioxidant, and 4-10 parts of softener; The butyl rubber is one or more of Exxon268, Xinhui 532, and Yanshan IIR1751; The filler is maleimide-grafted graphene and at least one of talc, kaolin, titanium dioxide, montmorillonite, mica powder, calcium carbonate, barium sulfate, worm graphite, aluminum oxide, magnesium oxide, and boron nitride; The polyisobutylene includes one or more of PB 680, PB1300, and PB2400; The tackifier includes one or more of petroleum resin, terpene resin, phenolic resin, and epoxy resin; The vulcanizing agent includes one or more of sulfur, colloidal sulfur, sulfur monochloride The carbon black includes one or more of N330, N774, and N990; The reinforcing agent includes one or more of fumed silica and precipitated silica; The dispersant includes at least one of a silane coupling agent, a stearate, and a titanate coupling agent; The antioxidant includes at least one of nano silicon nitride, phenolic antioxidant and heterocyclic antioxidant; The softener includes at least one of naphthenic oil, dibutyl ester and paraffin oil.

8. The butyl rubber damping material prepared by using the hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol composite material according to claim 7, characterized in that: The filler is maleimide-grafted graphene, mica powder with a sheet diameter less than 6.5 microns, and boron nitride nanosheets with a sheet diameter less than 500 nm, which are composed of a mass ratio of (5-20):(70-90):(5-10).

9. The butyl rubber damping material prepared by using the hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol composite material according to claim 7, characterized in that: The preparation method of maleimide-grafted graphene comprises the following steps: firstly, modifying hydroxylated graphene with an aminosilane coupling agent to obtain graphene with amino groups on the surface; then reacting maleimidopropionic acid with an acyl chloride reagent to produce maleimidopropionyl chloride; dissolving the obtained maleimidopropionyl chloride and graphene with amino groups on the surface in an acetone / DMF mixed solution, reacting at 60-80° C. for 3-5 hours, and after the reaction is completed, vacuum filtering the obtained solid matter and placing it under vacuum drying at 120-160° C. and 0.5-1.0 Pa for 4-6 hours to obtain maleimide-grafted graphene.

10. The butyl rubber damping material prepared by using the hydroxyl-terminated hyperbranched polyester graft-modified hindered phenol composite material according to claim 7, characterized in that: The preparation method of the butyl rubber damping material is as follows: Step 1, preparation of a hydroxyl-terminated hyperbranched polyester grafted modified hindered phenol composite material and maleimide grafted graphene; Step 2: Put the proportion of butyl rubber and the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite material into an internal mixer and mix them at 80-100° C. for 10 min; continue to add the proportion of tackifier, carbon black, reinforcing agent, vulcanizer, dispersant, antioxidant, and softener and continue to mix for 20 min; continue to add half of the proportion of filler and liquid polyisobutylene and continue to mix for 20 min; add the remaining half of the filler and liquid polyisobutylene and continue to mix for 30-50 min, discharge the material, and naturally cool it to room temperature to obtain the end-hydroxy hyperbranched polyester grafted modified hindered phenol composite butyl damping rubber.

Citation Information

Patent Citations

  • Modified hindered phenol damping agent, and preparation method and applications thereof

    CN105399961A

  • Hindered phenol / montmorillonoid / nitrile rubber composite damping material for car and preparing method thereof

    CN106543739A

  • Silicone rubber / hindered phenol composite modified butyl chloride damping rubber and preparation method thereof

    CN107629340A

  • Preparation method of chlorobutyl rubber compound damping material

    CN107815030A

  • Low-cost halloysite nanotube synergistic toughened aramid fiber and preparation method thereof

    CN108998851A

Cited By

  • Preparation method and application of hindered phenol quaternary phosphonium salt modified montmorillonite

    CN119191311A

  • Sound insulation carpet material composition, material and application of material in automotive trim

    CN121471626A