Medium-resistant high-elasticity rubber material for sealing element and preparation method of medium-resistant high-elasticity rubber material
By using materials such as nitrile rubber and preparation methods of modified polytetrafluoroethylene powder, the medium resistance and low-temperature performance of the seals are improved, and the performance degradation problem of rubber seals caused by oil and high temperature in mechanical equipment is solved. Extended service life.
Patent Information
- Application Number
- CN202411048917.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Rubber seals are easily affected by acid-base components and oil in the lubrication system of mechanical equipment, leading to expansion and performance degradation, and are damaged in high-temperature environments. Existing materials have insufficient media resistance and low-temperature performance.
Using ingredients such as nitrile rubber, modified polytetrafluoroethylene powder, trans-butadiene rubber, zinc oxide, stearic acid, antioxidant, spray carbon black, white carbon black, plasticizer and peroxide, through modification The preparation method and mixing process of polytetrafluoroethylene powder improve the medium resistance and low temperature performance of seals.
It significantly improves the medium resistance and low temperature cold resistance of the seal, extends the service life, reduces the dissolution and expansion of oil, and enhances the adaptability to high temperature environments.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sealing materials and relates to a medium-resistant high-elasticity rubber material for sealing components and a preparation method thereof. Background Art
[0002] Rubber seals are a common, fundamental component in sealing devices. They are a widely used rubber product in sealing technology. Due to their very low elastic modulus, high elongation, and excellent gas permeability, they are widely used in various mechanical equipment. However, the lubrication systems of mechanical equipment contain acids, bases, and oils, which can easily penetrate the seals, causing them to swell and shorten their service life. Furthermore, harsh operating environments, such as high temperatures, can damage the seals.
[0003] Medium resistance is the ability of a sealing material to resist changes in the physical properties and appearance of rubber caused by oil when it comes into contact with various oils. The sealing performance of the rubber sealing material is seriously affected after the volume and shape change. There are two main changes when the rubber is in contact with grease for a long time: First, the amount of oil molecules that penetrate into the rubber is greater than the amount of compounding agents precipitated, which will cause the volume of the rubber material to increase, thereby changing the sealing performance; second, the small molecule compounding agents in the rubber may dissolve in the oil solvent, resulting in a decrease in the volume of the rubber, and the extracted compounding agents may contaminate the oil. The longer the rubber sealing material is in contact with the oil, the more serious the swelling or precipitation. Therefore, it is necessary to change the polarity of the rubber sealing material, and the better the medium resistance by enhancing its polarity. However, the greater the polarity, the greater the intermolecular interaction force, resulting in poorer flexibility of the molecular chain and poorer low-temperature resistance. Therefore, the medium-resistant high-elasticity rubber material and preparation method for seals provided by the present invention can effectively solve the above problems. Summary of the Invention
[0004] The present invention relates to a medium-resistant high-elastic rubber material for seals and a preparation method thereof, and belongs to the technical field of sealing materials. The specific components of the medium-resistant high-elastic rubber material for seals disclosed in the present invention include nitrile rubber, modified polytetrafluoroethylene powder, trans-butadiene rubber, zinc oxide, stearic acid, antioxidant, spray carbon black, white carbon black, plasticizer, peroxide, and accelerator, wherein the preparation method of the modified polytetrafluoroethylene powder is: soaking the polytetrafluoroethylene powder in a treatment liquid, taking it out and drying it, which is the modified polytetrafluoroethylene powder. The modification of the polytetrafluoroethylene powder with the treatment liquid infiltrates into the interior of the powder, thereby improving the medium resistance of the seal. In addition, the low-temperature cold resistance of the seal is improved by adding spray carbon black, white carbon black and under the joint action of the plasticizer.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A medium-resistant high-elastic rubber material for a seal comprises the following raw materials: nitrile rubber, modified polytetrafluoroethylene powder, trans-butadiene rubber, zinc oxide, stearic acid, antioxidant, spray carbon black, white carbon black, plasticizer, peroxide, and accelerator.
[0007] Furthermore, the medium-resistant high-elasticity rubber material for the seal comprises the following raw materials in parts by weight: 70-80 parts of nitrile rubber, 40-50 parts of modified polytetrafluoroethylene powder, 10-15 parts of trans-butadiene rubber, 4-8 parts of zinc oxide, 1-2 parts of stearic acid, 1-2 parts of antioxidant, 20-40 parts of spray carbon black, 10-15 parts of
[0008] White carbon black, 4-5 parts of plasticizer, 1-2 parts of peroxide, 1-2 parts of accelerator.
[0009] Furthermore, the preparation method of the modified polytetrafluoroethylene powder comprises the following steps:
[0010] (1) Methyl acrylate, butyl methacrylate and No. 120 gasoline are stirred and mixed, and then benzoyl peroxide as an initiator is added and mixed to obtain a treatment liquid;
[0011] (2) Taking polytetrafluoroethylene powder and immersing it in the treatment liquid, filtering and separating it, and drying the solid to obtain modified polytetrafluoroethylene powder.
[0012] Furthermore, in the step (1), the volume ratio of methyl acrylate, butyl methacrylate and No. 120 gasoline is 3.5-4:1:5, and the amount of benzoyl peroxide added accounts for 5-8% of the mass of the treated liquid.
[0013] Furthermore, the immersion time in step (2) is 30-60 minutes, and the drying temperature and time are 50-70° C. and 2-3 hours, respectively.
[0014] A method for preparing a medium-resistant and highly elastic rubber material for a seal, the method comprising the following steps:
[0015] A1: Nitrile rubber, modified polytetrafluoroethylene powder, and trans-butadiene rubber are placed in an internal mixer and heated. Zinc oxide, stearic acid, an antioxidant, spray carbon black, and white carbon black are then added in sequence and mixed. The mixture is discharged to obtain mixture a.
[0016] A2: Mixture a is put into an open mill, and a plasticizer, a peroxide, and an accelerator are added, mixed, and cooled to obtain a medium-resistant and highly elastic rubber material for seals.
[0017] Furthermore, the temperature of the heating in step A1 is 100-150° C., and the mixing time and temperature are 20-30 min and 150-200° C., respectively.
[0018] Furthermore, in the step A2, the mixing time and temperature are 10-20 min and 100-150° C., respectively; the plasticizer is dioctyl phthalate; the peroxide is cyclohexanone peroxide; and the accelerator is accelerator DM.
[0019] Beneficial effects of the present invention:
[0020] 1. The treatment liquid is used to modify polytetrafluoroethylene. Under the action of the drying temperature, condensation and polymerization reactions occur, leaving methyl acrylate and butyl methacrylate in the pores of polytetrafluoroethylene, thereby enhancing the material's media resistance. At the same time, the synergistic effect of the treatment liquid with nitrile rubber and trans-butadiene rubber further enhances the material's media resistance.
[0021] 2. The low temperature resistance of the seal is improved by adding spray carbon black, white carbon black and the combined effect of plasticizers. DETAILED DESCRIPTION
[0022] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0023] Example 1
[0024] A medium-resistant high-elastic rubber material for a seal comprises the following raw materials: nitrile rubber, modified polytetrafluoroethylene powder, trans-butadiene rubber, zinc oxide, stearic acid, antioxidant, spray carbon black, white carbon black, plasticizer, peroxide, and accelerator.
[0025] Furthermore, the medium-resistant high-elasticity rubber material for the seal includes the following raw materials in parts by weight: 70 parts of nitrile rubber, 40 parts of modified polytetrafluoroethylene powder, 10 parts of trans-butadiene rubber, 4 parts of zinc oxide, 1 part of stearic acid, 1 part of antioxidant, 20 parts of spray carbon black, 10 parts of white carbon black, 4 parts of plasticizer, 1 part of peroxide, and 1 part of accelerator.
[0026] The preparation method of the modified polytetrafluoroethylene powder comprises the following steps:
[0027] (1) Methyl acrylate, butyl methacrylate and No. 120 gasoline are stirred and mixed, and then benzoyl peroxide as an initiator is added and mixed to obtain a treatment liquid;
[0028] (2) Taking polytetrafluoroethylene powder and immersing it in the treatment liquid, filtering and separating it, and drying the solid to obtain modified polytetrafluoroethylene powder.
[0029] In the step (1), the volume ratio of methyl acrylate, butyl methacrylate and No. 120 gasoline is 3.5:1:5, and the amount of benzoyl peroxide added accounts for 5% of the mass of the treated liquid.
[0030] The immersion time in step (2) is 30 minutes, and the drying temperature and time are 50° C. and 2 hours, respectively.
[0031] A method for preparing a medium-resistant and highly elastic rubber material for a seal, the method comprising the following steps:
[0032] A1: Nitrile rubber, modified polytetrafluoroethylene powder, and trans-butadiene rubber are placed in an internal mixer and heated. Zinc oxide, stearic acid, an antioxidant, spray carbon black, and white carbon black are then added in sequence and mixed. The mixture is discharged to obtain mixture a.
[0033] A2: Mixture a is put into an open mill, and a plasticizer, a peroxide, and an accelerator are added, mixed, and cooled to obtain a medium-resistant and highly elastic rubber material for seals.
[0034] The temperature in step A1 is 100° C., and the mixing time and temperature are 20 min and 150° C., respectively.
[0035] The mixing time and temperature in step A2 are 10 min and 100° C., respectively. The plasticizer is dioctyl phthalate, the peroxide is cyclohexanone peroxide, and the accelerator is accelerator DM.
[0036] The antioxidant was purchased from Changchun-BPA, the spray carbon black was purchased from Baochi-1333-86-4, and the white carbon black was purchased from Shuangying-10279-57-9.
[0037] Example 2
[0038] A medium-resistant high-elastic rubber material for a seal comprises the following raw materials: nitrile rubber, modified polytetrafluoroethylene powder, trans-butadiene rubber, zinc oxide, stearic acid, antioxidant, spray carbon black, white carbon black, plasticizer, peroxide, and accelerator.
[0039] The medium-resistant high-elasticity rubber material for the seal includes the following raw materials in parts by weight: 75 parts of nitrile rubber, 45 parts of modified polytetrafluoroethylene powder, 12 parts of trans-butadiene rubber, 6 parts of zinc oxide, 1.5 parts of stearic acid, 1.5 parts of antioxidant, 30 parts of spray carbon black, 13 parts of white carbon black, 4.5 parts of plasticizer, 1.5 parts of peroxide, and 1.5 parts of accelerator.
[0040] The preparation method of the modified polytetrafluoroethylene powder comprises the following steps:
[0041] (1) Methyl acrylate, butyl methacrylate and No. 120 gasoline are stirred and mixed, and then benzoyl peroxide as an initiator is added and mixed to obtain a treatment liquid;
[0042] (2) Taking polytetrafluoroethylene powder and immersing it in the treatment liquid, filtering and separating it, and drying the solid to obtain modified polytetrafluoroethylene powder.
[0043] In the step (1), the volume ratio of methyl acrylate, butyl methacrylate and No. 120 gasoline is 3.8:1:5, and the amount of benzoyl peroxide added accounts for 6.5% of the mass of the treated liquid.
[0044] The immersion time in step (2) is 45 minutes, and the drying temperature and time are 60° C. and 2.5 hours, respectively.
[0045] A method for preparing a medium-resistant and highly elastic rubber material for a seal, the method comprising the following steps:
[0046] A1: Nitrile rubber, modified polytetrafluoroethylene powder, and trans-butadiene rubber are placed in an internal mixer and heated. Zinc oxide, stearic acid, an antioxidant, spray carbon black, and white carbon black are then added in sequence and mixed. The mixture is discharged to obtain mixture a.
[0047] A2: Mixture a is put into an open mill, and a plasticizer, a peroxide, and an accelerator are added, mixed, and cooled to obtain a medium-resistant and highly elastic rubber material for seals.
[0048] The temperature of the heating in step A1 is 125° C., and the mixing time and temperature are 25 min and 175° C., respectively.
[0049] The mixing time and temperature in step A2 are 15 minutes and 125° C., respectively. The plasticizer is dioctyl phthalate, the peroxide is cyclohexanone peroxide, and the accelerator is accelerator DM.
[0050] The antioxidant was purchased from Changchun-BPA, the spray carbon black was purchased from Baochi-1333-86-4, and the white carbon black was purchased from Shuangying-10279-57-9.
[0051] Example 3
[0052] A medium-resistant high-elastic rubber material for a seal comprises the following raw materials: nitrile rubber, modified polytetrafluoroethylene powder, trans-butadiene rubber, zinc oxide, stearic acid, antioxidant, spray carbon black, white carbon black, plasticizer, peroxide, and accelerator.
[0053] The medium-resistant high-elasticity rubber material for the seal includes the following raw materials in parts by weight: 80 parts of nitrile rubber, 50 parts of modified polytetrafluoroethylene powder, 15 parts of trans-butadiene rubber, 8 parts of zinc oxide, 2 parts of stearic acid, 2 parts of antioxidant, 40 parts of spray carbon black, 15 parts of white carbon black, 5 parts of plasticizer, 2 parts of peroxide, and 2 parts of accelerator.
[0054] The preparation method of the modified polytetrafluoroethylene powder comprises the following steps:
[0055] (1) Methyl acrylate, butyl methacrylate and No. 120 gasoline are stirred and mixed, and then benzoyl peroxide as an initiator is added and mixed to obtain a treatment liquid;
[0056] (2) Taking polytetrafluoroethylene powder and immersing it in the treatment liquid, filtering and separating it, and drying the solid to obtain modified polytetrafluoroethylene powder.
[0057] In the step (1), the volume ratio of methyl acrylate, butyl methacrylate and No. 120 gasoline is 4:1:5, and the amount of benzoyl peroxide added accounts for 8% of the mass of the treated liquid.
[0058] The immersion time in step (2) is 60 minutes, and the drying temperature and time are 70° C. and 3 hours, respectively.
[0059] A method for preparing a medium-resistant and highly elastic rubber material for a seal, the method comprising the following steps:
[0060] A1: Nitrile rubber, modified polytetrafluoroethylene powder, and trans-butadiene rubber are placed in an internal mixer and heated. Zinc oxide, stearic acid, an antioxidant, spray carbon black, and white carbon black are then added in sequence and mixed. The mixture is discharged to obtain mixture a.
[0061] A2: Mixture a is put into an open mill, and a plasticizer, a peroxide, and an accelerator are added, mixed, and cooled to obtain a medium-resistant and highly elastic rubber material for seals.
[0062] The temperature in step A1 is 150° C., and the mixing time and temperature are 30 min and 200° C., respectively.
[0063] The mixing time and temperature in step A2 are 20 min and 150° C., respectively. The plasticizer is dioctyl phthalate, the peroxide is cyclohexanone peroxide, and the accelerator is accelerator DM.
[0064] The antioxidant was purchased from Changchun-BPA, the spray carbon black was purchased from Baochi-1333-86-4, and the white carbon black was purchased from Shuangying-10279-57-9.
[0065] Comparative Example 1
[0066] Based on Example 3, a medium-resistant high-elastic rubber material for seals is provided, which includes the following raw materials: nitrile rubber, polytetrafluoroethylene powder, trans-butadiene rubber, zinc oxide, stearic acid, antioxidant, spray carbon black, white carbon black, plasticizer, peroxide, and accelerator.
[0067] The medium-resistant high-elasticity rubber material for the seal includes the following raw materials in parts by weight: 80 parts of nitrile rubber, 50 parts of polytetrafluoroethylene powder, 15 parts of trans-butadiene rubber, 8 parts of zinc oxide, 2 parts of stearic acid, 2 parts of antioxidant, 40 parts of spray carbon black, 15 parts of white carbon black, 5 parts of plasticizer, 2 parts of peroxide, and 2 parts of accelerator.
[0068] A method for preparing a medium-resistant and highly elastic rubber material for a seal, the method comprising the following steps:
[0069] A1: Nitrile rubber, polytetrafluoroethylene powder, and trans-butadiene rubber are placed in an internal mixer and heated. Zinc oxide, stearic acid, an antioxidant, spray carbon black, and white carbon black are then added in sequence and mixed. The mixture is discharged to obtain a mixture a.
[0070] A2: Mixture a is put into an open mill, and a plasticizer, a peroxide, and an accelerator are added, mixed, and cooled to obtain a medium-resistant and highly elastic rubber material for seals.
[0071] The temperature in step A1 is 150° C., and the mixing time and temperature are 30 min and 200° C., respectively.
[0072] The mixing time and temperature in step A2 are 20 min and 150° C., respectively. The plasticizer is dioctyl phthalate, the peroxide is cyclohexanone peroxide, and the accelerator is accelerator DM.
[0073] The antioxidant was purchased from Changchun-BPA, the spray carbon black was purchased from Baochi-1333-86-4, and the white carbon black was purchased from Shuangying-10279-57-9.
[0074] Comparative Example 2
[0075] On the basis of Example 3, the seal is removed and the spray carbon black in the raw material for preparing the medium-resistant high-elasticity rubber material is replaced with an equal weight portion of white carbon black. Other conditions are consistent with Example 3.
[0076] Comparative Example 3
[0077] On the basis of Example 3, the sealing member is removed and the white carbon black in the raw material for preparing the medium-resistant high-elasticity rubber material is replaced with an equal weight portion of spray carbon black. Other conditions are the same as those in Example 3.
[0078] Comparative Example 4
[0079] On the basis of Example 3, the plasticizer in the raw material for preparing the medium-resistant high-elasticity rubber material for the seal is removed and replaced with an equal weight portion of white carbon black. Other conditions are consistent with Example 3.
[0080] 1. Performance Testing
[0081] The medium-resistant high-elasticity rubber materials obtained in Examples 1-3 and Comparative Examples 1-4 were made into standard splines with a specification of 2cm×2cm×4cm. The compression cold resistance coefficient of the splines was tested according to GB / T6034-1985, and the medium resistance performance of the splines was tested according to GB / T1690-2010. Specifically, the splines were immersed in lubricating oil at a temperature of 100°C for 24 hours and then taken out to test the volume change rate of the test sample before and after oil immersion.
[0082] The above test results are shown in Table 1:
[0083] Table 1 Molecular weight test results
[0084] Sample Compression cold resistance coefficient / 50℃ Volume change rate% Example 1 0.42 2.56 Example 2 0.40 3.74 Example 3 0.42 3.91 Comparative Example 1 - 12.47 Comparative Example 2 0.28 - Comparative Example 3 0.30 - Comparative Example 4 0.27 -
[0085] As can be seen from Table 1, the compression cold resistance coefficients of Examples 1-3 are greater than those of Comparative Examples 2-4, and the volume change rates are less than those of Comparative Example 1. The polytetrafluoroethylene powder in the comparative examples was not soaked in the treatment liquid, resulting in poor media resistance. In Comparative Examples 2-4, the cold resistance effect was reduced by removing one of the spray carbon black, white carbon black, and plasticizer.
[0086] The above description is merely a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as above in terms of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art can, without departing from the scope of the technical solution of the present invention, make some changes or modifications to equivalent embodiments using the technical contents disclosed above. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A medium-resistant high-elastic rubber material for a seal, characterized in that: The medium-resistant high-elastic rubber material for the seal comprises the following raw materials: nitrile rubber, modified polytetrafluoroethylene powder, trans-butadiene rubber, zinc oxide, stearic acid, antioxidant, spray carbon black, white carbon black, plasticizer, peroxide, and accelerator.
2. The medium-resistant high-elastic rubber material for a seal according to claim 1, characterized in that: The medium-resistant high-elastic rubber material for the seal comprises the following raw materials in parts by weight: 70-80 parts of nitrile rubber, 40-50 parts of modified polytetrafluoroethylene powder, 10-15 parts of trans-butadiene rubber, 4-8 parts of zinc oxide, 1-2 parts of stearic acid, 1-2 parts of antioxidant, 20-40 parts of spray carbon black, 10-15 parts of white carbon black, 4-5 parts of plasticizer, 1-2 parts of peroxide, and 1-2 parts of accelerator.
3. The medium-resistant high-elastic rubber material for a seal according to claim 1, characterized in that: The preparation method of the modified polytetrafluoroethylene powder comprises the following steps: (1) Methyl acrylate, butyl methacrylate and No. 120 gasoline are stirred and mixed, and then an initiator benzoyl peroxide is added and mixed to obtain a treatment liquid; (2) taking polytetrafluoroethylene powder and immersing it in the treatment liquid, filtering and separating the powder, and drying the solid to obtain modified polytetrafluoroethylene powder.
4. The medium-resistant high-elastic rubber material for a seal according to claim 3, characterized in that: In the step (1), the volume ratio of methyl acrylate, butyl methacrylate and No. 120 gasoline is 3.5-4:1:5, and the amount of benzoyl peroxide added accounts for 5-8% of the mass of the treated liquid.
5. The medium-resistant high-elastic rubber material for a seal according to claim 3, characterized in that: The immersion time in step (2) is 30-60 minutes, and the drying temperature and time are 50-70° C. and 2-3 hours, respectively.
6. A method for preparing the medium-resistant high-elastic rubber material for seals according to any one of claims 1 to 5, characterized in that: The method for preparing the medium-resistant high-elastic rubber material for the seal comprises the following steps: A1: Put nitrile rubber, modified polytetrafluoroethylene powder and trans-butadiene rubber into an internal mixer and heat them up, then add zinc oxide, stearic acid, antioxidant, spray carbon black and white carbon black in sequence for mixing, and discharge to obtain a mixture a; A2: Mixture a is put into an open mill, and a plasticizer, a peroxide and an accelerator are added, mixed, and after cooling, a medium-resistant and highly elastic rubber material for a seal is obtained.
7. The method for preparing a medium-resistant high-elastic rubber material for a seal according to claim 6, characterized in that: The temperature of the heating in step A1 is 100-150° C., and the mixing time and temperature are 20-30 min and 150-200° C. respectively.
8. The method for preparing a medium-resistant high-elastic rubber material for a seal according to claim 6, characterized in that: The mixing time and temperature in step A2 are 10-20 min and 100-150° C. respectively, the plasticizer is dioctyl phthalate, the peroxide is cyclohexanone peroxide, and the accelerator is accelerator DM.
Citation Information
Patent Citations
Butadiene-acrylonitrile rubber material for oil seal of washing machine
CN106750648A
Oil-resistant high-temperature-resistant low-friction-coefficient tooth cloth glue as well as preparation method and application thereof
CN114539647A
Oil-resistant rubber gasket, preparation method and high-strength oil-resistant rubber expansion joint
CN115558175A
Medium-resistant modified expanded polytetrafluoroethylene sealing material
CN115819822A
Cited By
Solvent-resistant foaming material and preparation method thereof
CN120818187A