Warm mixing regenerant, asphalt mixture and preparation method of warm mixing regenerant

By adding modified polymer emulsion, nano-titanium dioxide, waste rubber powder and recycled oil to the asphalt mixture, and using basalt or limestone, the problems of high heat absorption and easy cracking of traditional asphalt mixtures are solved, and the heat absorption is reduced. properties, improve self-healing and water permeability, and extend the life of the road.

CN118725499AInactive Publication Date: 2024-10-01Jiangxi Jiaotong Maintenance Technology Group Co., Ltd.

Patent Information

Application Number
CN202410959157.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Due to high heat absorption and easy cracking of traditional asphalt mixtures, the urban heat island effect is aggravated and roads are damaged, which increases maintenance costs and traffic management pressure.

Method used

A warm-mix regeneration agent is used, including modified polymer emulsion, nano-titanium dioxide, waste rubber powder and recycled oil, and an asphalt mixture preparation method that reduces heat absorption and improves self-healing capabilities is combined with basalt or limestone as mineral materials to form porous Structure to improve water permeability.

Benefits of technology

It significantly reduces the heat absorption of asphalt mixture, improves its self-healing ability and water permeability, extends the service life of roads, reduces maintenance costs and environmental pollution, and alleviates the heat island effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725499A_ABST
    Figure CN118725499A_ABST
Patent Text Reader

Abstract

The invention discloses a warm mixing regenerant, an asphalt mixture and a preparation method of the warm mixing regenerant, and relates to the technical field of road engineering materials, and the warm mixing regenerant is technically characterized by comprising the following components in percentage by weight: 10-20% of modified polymer emulsion, 2-5% of nano titanium dioxide, 5-10% of waste rubber powder, 10-20% of regenerated oil and the balance of solvent, the invention has the technical effects that the nano technology is introduced to endow the traditional warm-mixing regenerant with new performance, specifically, nano titanium dioxide is ingeniously added into the warm-mixing regenerant, the reflection performance of the material is remarkably improved by the measure, and further a remarkable heat absorptivity reduction effect is brought to the asphalt mixture; the introduction of the nano titanium dioxide is not simple physical mixing, the unique particle structure of the nano titanium dioxide forms a fine and uniform reflecting layer on the surface of the asphalt, and the reflecting layer is like a natural sunshade and can efficiently reflect solar radiation back to the atmosphere.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road engineering materials, in particular to a warm mix regeneration agent, an asphalt mixture and a preparation method thereof. Background Art

[0002] Against the backdrop of global warming, the urban heat island effect has become increasingly prominent, which has put considerable pressure on the urban environment. Traditional asphalt mixtures, due to their inherent high heat absorption characteristics, not only exacerbate the temperature rise on the urban surface, but also further deteriorate the urban microclimate, bringing many negative impacts on the quality of life of residents and the urban ecological environment;

[0003] What is more serious is that traditional asphalt pavement is easily affected by various factors during long-term use, such as temperature changes, vehicle loads, etc., which can cause cracks and damage to the pavement. These cracks not only affect the flatness and driving safety of the road, but also increase the maintenance cost of the pavement, bringing considerable pressure to urban traffic management and public finances.

[0004] Therefore, developing an asphalt mixture with low heat absorption and self-healing ability has become an urgent problem to be solved in the current urban construction and transportation development. This new asphalt mixture can not only effectively reduce the temperature of the urban surface and alleviate the heat island effect, but also automatically fill the road cracks through its own self-healing mechanism, extend the service life of the road, and reduce maintenance costs. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a warm mix regeneration agent, an asphalt mixture and a preparation method thereof, which can reduce the heat absorption performance of the asphalt mixture and improve the self-repairing ability of the asphalt mixture.

[0007] (II) Technical solution

[0008] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a warm mix regeneration agent, asphalt mixture and preparation method thereof, comprising the following components by weight percentage: 10-20% modified polymer emulsion, 2-5% nano titanium dioxide, 5-10% waste rubber powder, 10-20% recycled oil and 45-60% solvent.

[0009] Preferably, the modified polymer emulsion is styrene-butadiene-styrene (SBS) copolymer.

[0010] Preferably, the particle size of the nano titanium dioxide is 20-50 nanometers.

[0011] Preferably, the waste rubber powder comes from waste tires.

[0012] Preferably, the regenerated oil is a mixture of vegetable oil and mineral oil, and the ratio of the two is (4-7): (10-11).

[0013] Preferably, the base asphalt is 80-90%, the warm mix regeneration agent is 5-6%, and the mineral material is 3-5%.

[0014] Preferably, the base asphalt is road petroleum asphalt.

[0015] Preferably, the mineral material is basalt or limestone aggregate.

[0016] The method for preparing asphalt mixture comprises the following steps:

[0017] S1: Raw material preparation: prepare the base asphalt, warm mix regeneration agent and mineral materials in proportion;

[0018] S2: Preparation of warm mix regeneration agent, mixing the modified polymer emulsion, nano titanium dioxide, waste rubber powder and recycled oil in proportion;

[0019] S3: Asphalt mixture preparation: add warm mix regeneration agent into base asphalt, heat to 140-160℃, and stir evenly;

[0020] S4: Warm mix, adding mineral material to the heated asphalt mixture and mixing at 120-140°C;

[0021] S5: Mixture shaping and compacting: pouring the mixture into a mold and compacting it;

[0022] S6: Cooling and curing: cooling the formed mixture at room temperature and curing.

[0023] (III) Beneficial effects

[0024] Compared with the prior art, the present invention provides a warm mix regeneration agent, asphalt mixture and a preparation method thereof, which have the following beneficial effects:

[0025] 1. In pursuit of more efficient and environmentally friendly road construction solutions, nano titanium dioxide is added to warm mix regeneration agents, which significantly improves the reflective properties of the material, thereby significantly reducing the heat absorption of asphalt mixtures;

[0026] The introduction of nano-titanium dioxide is not a simple physical mixture. Its unique particle structure forms a fine and uniform reflective layer on the asphalt surface. This reflective layer is like a natural parasol, which can efficiently reflect solar radiation back into the atmosphere instead of being absorbed by the asphalt. This not only effectively reduces the asphalt's absorption of heat from sunlight, but also greatly reduces the temperature of the road surface, thereby slowing down the aging of the asphalt and extending the service life of the road surface.

[0027] In addition, the addition of nano-titanium dioxide also brings many additional benefits. For example, its excellent photocatalytic performance helps decompose pollutants on the road surface and reduce the environmental burden; at the same time, the small size effect of nano-materials also enhances the bonding force between asphalt and aggregate, improving the shear strength and durability of the road surface;

[0028] In conclusion, by adding nano-titanium dioxide to warm mix regeneration agent, we can not only obtain asphalt mixture with excellent reflective properties, but also effectively reduce the pavement temperature and improve the service life and environmental performance of the pavement.

[0029] 2. When we cleverly combine recycled oil and waste rubber powder, we are actually giving asphalt mixture an unprecedented self-healing ability. This unique combination can respond quickly and effectively when cracks appear, thus ensuring the durability and safety of the road;

[0030] Specifically, when tiny cracks quietly appear on the asphalt pavement, the flowable components in the recycled oil will be quickly activated. These components have excellent fluidity and can quickly penetrate deep into the cracks, laying a solid foundation for subsequent repair work. At the same time, the elastic properties of waste rubber powder also play a key role. They can not only form a layer of elastic filler at the cracks, but also interact with the components in the recycled oil to form a strong and flexible repair layer.

[0031] The introduction of this self-healing ability has greatly improved the overall performance of asphalt mixtures. It can not only repair cracks in time at the early stage to prevent further expansion of cracks, but also improve the durability and service life of the road surface. In addition, since this repair process is automatic and does not require human intervention, it also greatly reduces maintenance costs and manpower investment.

[0032] 3. In the preparation process of asphalt mixture, the use of basalt or limestone as mineral components not only brings significant performance improvement to road construction, but also demonstrates the perfect combination of environmental protection and practicality. The use of these two minerals can cleverly form a porous structure, thereby greatly improving the permeability of asphalt mixture;

[0033] Basalt and limestone play a key role in asphalt mixtures with their unique physical properties, such as high hardness, wear resistance and excellent chemical stability. Their surface roughness allows asphalt to adhere more tightly to the mineral particles, forming a more stable structure. At the same time, the porosity of these minerals also provides good infiltration channels for water, significantly improving the permeability of the mixture.

[0034] By using basalt or limestone as mineral materials, the water permeability of asphalt mixture has been greatly improved. In the rainy season or when there is heavy rainfall, the water on the road surface can be quickly discharged through the pores in the mixture, effectively reducing the phenomenon of water accumulation on the road surface. This not only improves the road's traffic capacity and driving safety, but also helps to keep the road clean and reduce the generation of water mist, thereby improving the road's driving environment;

[0035] In addition, the porous asphalt mixture also has good environmental performance. It can absorb and store rainwater, reduce the impact of rainwater runoff on the environment, and help maintain the ecological balance. At the same time, this structure can also reduce the road surface temperature and reduce the occurrence of urban heat island effect.

[0036] 4. In the preparation of asphalt mixture, the introduction of SBS (styrene-butadiene-styrene) modified polymer emulsion, this advanced modified material not only significantly enhances the anti-aging performance of asphalt mixture, but also greatly improves its wear resistance, thus ensuring a longer service life and higher stability of the road surface;

[0037] SBS modified polymer emulsion forms a tough and durable protective layer by closely combining with asphalt mixture. This protective layer can effectively resist aging caused by natural factors such as ultraviolet rays, high temperature, oxidation, etc., so that the asphalt mixture can still maintain excellent performance during long-term use;

[0038] At the same time, the addition of SBS modified polymer emulsion also significantly improves the wear resistance of asphalt mixture. During the driving process, the road surface will be frequently subjected to friction and wear, but the presence of SBS modified polymer emulsion can significantly reduce this wear, maintain the flatness and anti-skid properties of the road surface, and ensure driving safety;

[0039] In addition, SBS modified polymer emulsion also has excellent adhesion and compatibility, and can be fully integrated with other components in asphalt mixture to form a composite material with superior overall performance. The use of this composite material not only improves the service life and stability of the road surface, but also brings new development opportunities to the field of road construction. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 The invention is a flow chart of a warm mix regeneration agent, an asphalt mixture and a preparation method thereof. DETAILED DESCRIPTION

[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0042] The present invention uses recycled oil and waste rubber powder as raw materials, which convert waste into valuable resources through recycling. Recycled oil, which comes from waste grease or other organic matter, can be used to manufacture building materials such as asphalt mixture after refining and treatment, effectively reducing the dependence on new oil resources. Waste rubber powder is a particulate material obtained by crushing and processing rubber products such as waste tires. Its unique elasticity and wear resistance make it an ideal additive to enhance the performance of asphalt mixture. By combining recycled oil and waste rubber powder, we can not only reduce the pollution of waste to the environment, but also improve the performance of building materials and promote the development of green buildings.

[0043] Basalt and limestone are used as raw materials. As two common igneous rocks, they not only occupy an important position in geological structures, but also show excellent practical value in the fields of architecture and engineering. They are derived from the cooling and solidification of high-temperature magma deep in the earth, so they have extremely high hardness and durability. Basalt, with its dark appearance and delicate texture, is often used in paving stones, building materials and decorative stones, adding natural beauty to the urban landscape. Limestone, with its hard and wear-resistant characteristics, is widely used in building foundations, road paving and monument production, and has withstood the test of time.

[0044] The use of SBS (styrene-butadiene-styrene) modified polymer emulsion as raw material has brought revolutionary changes to asphalt mixture and other building materials with its unique molecular structure and excellent performance. This emulsion is synthesized by copolymerization of three monomers: styrene, butadiene and styrene. It has excellent elasticity and wear resistance, and can effectively improve the anti-aging performance and stability of asphalt mixture. The addition of SBS modified polymer emulsion not only significantly enhances the durability of asphalt mixture, but also improves its low-temperature crack resistance and fatigue resistance, making the road safer and more durable. In addition, SBS modified polymer emulsion also has excellent compatibility and processability, and can be fully integrated with asphalt mixture to form a uniform and stable composite material.

[0045] Embodiment 1:

[0046] A warm mix regeneration agent, asphalt mixture and a preparation method thereof, specifically comprising the following steps:

[0047] S1. Preparation of warm-mix regeneration agent: 15 g of modified polymer emulsion (SBS), 3 g of nano titanium dioxide, 7 g of waste rubber powder, 15 g of regenerated oil and 50 g of solvent were mixed uniformly in proportion to obtain a warm-mix regeneration agent;

[0048] S2. Raw material preparation: 85g base asphalt, 5.5g warm mix regeneration agent, 3.5g mineral material;

[0049] S3. Preparation of asphalt mixture: Add warm mix regeneration agent into base asphalt, heat to 150°C, and stir evenly;

[0050] S4, warm mix: adding the mineral material to the heated asphalt mixture and mixing at 130°C;

[0051] S5, mixture molding and compaction: pouring the mixture into a mold and compacting it;

[0052] S6. Cooling and curing: The formed mixture is cooled at room temperature and cured.

[0053] Embodiment 2:

[0054] A warm mix regeneration agent, asphalt mixture and a preparation method thereof, specifically comprising the following steps:

[0055] S1. Preparation of warm-mix regeneration agent: 15 g of modified polymer emulsion (SBS), 3 g of nano titanium dioxide, 7 g of waste rubber powder, 15 g of regenerated oil and 50 g of solvent were mixed uniformly in proportion to obtain a warm-mix regeneration agent;

[0056] S2. Raw material preparation: 85g of base asphalt, 5.5g of warm mix regeneration agent, and 5g of mineral material;

[0057] S3. Preparation of asphalt mixture: Add warm mix regeneration agent into base asphalt, heat to 150°C, and stir evenly;

[0058] S4, warm mix: adding the mineral material to the heated asphalt mixture and mixing at 130°C;

[0059] S5, mixture molding and compaction: pouring the mixture into a mold and compacting it;

[0060] S6. Cooling and curing: The formed mixture is cooled at room temperature and cured.

[0061] Embodiment three:

[0062] A warm mix regeneration agent, asphalt mixture and a preparation method thereof, specifically comprising the following steps:

[0063] S1. Preparation of warm mix regeneration agent: 18 g of modified polymer emulsion (SBS), 2 g of nano titanium dioxide, 7 g of waste rubber powder, 13 g of regenerated oil and 50 g of solvent were mixed uniformly in proportion;

[0064] S2. Raw material preparation: 83g of base asphalt, 12g of warm mix regeneration agent, and 5g of mineral material;

[0065] S3. Preparation of asphalt mixture: Add warm mix regeneration agent into base asphalt, heat to 145°C, and stir evenly;

[0066] S4, warm mix: adding the mineral material to the heated asphalt mixture and mixing at 125°C;

[0067] S5, mixture molding and compaction: pouring the mixture into a mold and compacting it;

[0068] S6. Cooling and curing: The formed mixture is cooled at room temperature and cured.

[0069] Embodiment 4:

[0070] A warm mix regeneration agent, asphalt mixture and a preparation method thereof, specifically comprising the following steps:

[0071] S1. Preparation of warm mix regeneration agent: 15 g of modified polymer emulsion (SBS), 3 g of nano titanium dioxide, 6 g of waste rubber powder, 16 g of regenerated oil and 50 g of solvent were mixed evenly in proportion;

[0072] S2. Raw material preparation: 82g of base asphalt, 5.5g of warm mix regeneration agent, and 8g of mineral material;

[0073] S3. Preparation of asphalt mixture: Add warm mix regeneration agent into base asphalt, heat to 150°C, and stir evenly;

[0074] S4, warm mix: adding the mineral material to the heated asphalt mixture and mixing at 130°C;

[0075] S5, mixture molding and compaction: pouring the mixture into a mold and compacting it;

[0076] S6. Cooling and curing: The formed mixture is cooled at room temperature and cured.

[0077] Embodiment five:

[0078] A warm mix regeneration agent, asphalt mixture and a preparation method thereof, specifically comprising the following steps:

[0079] S1. Preparation of warm mix regeneration agent: 15 g of modified polymer emulsion (SBS), 3 g of nano titanium dioxide, 6 g of waste rubber powder, 15 g of regenerated oil and 50 g of solvent were mixed evenly in proportion;

[0080] S2. Raw material preparation: 85g of base asphalt, 5.5g of warm mix regeneration agent, and 5g of mineral material;

[0081] S3. Preparation of asphalt mixture: Add warm mix regeneration agent into base asphalt, heat to 150°C, and stir evenly;

[0082] S4, warm mix: adding the mineral material to the heated asphalt mixture and mixing at 130°C;

[0083] S5, mixture molding and compaction: pouring the mixture into a mold and compacting it;

[0084] S6. Cooling and curing: The formed mixture is cooled at room temperature and cured.

[0085] Comparative Example 1:

[0086] S1. Raw material preparation: 85g base asphalt, non-warm mix regeneration agent, 5g mineral material;

[0087] S2. Preparation of asphalt mixture: heat the base asphalt to 160°C and stir evenly;

[0088] S3, warm mix: adding the mineral material to the heated asphalt mixture and mixing at 150°C;

[0089] S4, mixture molding and compaction: pouring the mixture into a mold and compacting it;

[0090] S5. Cooling and curing: The formed mixture is cooled at room temperature and cured.

[0091] Comparative Example 2:

[0092] S1. Raw material preparation: 90g of base asphalt, non-warm mix regeneration agent, 10g of mineral material;

[0093] S2. Preparation of asphalt mixture: heat the base asphalt to 160°C and stir evenly;

[0094] S3, warm mix: adding the mineral material to the heated asphalt mixture and mixing at 150°C;

[0095] S4, mixture molding and compaction: pouring the mixture into a mold and compacting it;

[0096] S5. Cooling and curing: The formed mixture is cooled at room temperature and cured.

[0097] The heat absorption performance of seven groups of asphalt mixtures in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 was tested. The testing method is as follows: the asphalt mixture samples prepared in each example and comparative example are placed in the sun for 1 hour, and the surface temperature is measured using an infrared thermometer to obtain an average value. The higher the temperature of the test result, the faster the heat absorption, and vice versa, the lower the temperature of the test result, the slower the heat absorption. The heat absorption performance test results are shown in Table 1. Therefore, by adding nano titanium dioxide to the warm mix regeneration agent, the material can effectively reduce the heat absorption of the asphalt mixture.

[0098] Table 1. Test results of heat absorption performance of Examples 1-5 and Comparative Examples 1-2

[0099]

[0100]

[0101] The water permeability test was performed on seven groups of asphalt mixtures in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2. The testing method is as follows: placing the asphalt mixture samples prepared in each example and comparative example in a water permeability testing device, measuring the amount of water passing through the sample per unit time, using a JGT376-D-ZD fully automatic water permeability tester, and testing the water permeability of the asphalt mixture by program-controlled water flow rates simulating light rain to heavy rain, or a simulation test with the same test requirements, the higher the value of the test result, the better the water permeability, and conversely, the higher the value of the test result, the worse the water permeability. The water permeability test results are shown in Table 2. Therefore, the use of basalt or limestone in the mineral material can form a porous structure and improve the water permeability of the asphalt mixture.

[0102] Table 2. Test results of water permeability of Examples 1-5 and Comparative Examples 1-2

[0103] Test samples <![CDATA[Water permeability (L / m 2 ·h)]]> Example 1 25 Example 2 24 Example 3 26 Example 4 23 Example 5 25 Comparative Example 1 10 Comparative Example 2 12

[0104] The self-repairing ability of seven groups of asphalt mixtures in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 was tested. The testing method was to create cracks of the same degree on the asphalt mixture samples prepared in each example and comparative example, and measure the healing time of the cracks. The shorter the crack healing time in the test results, the better the self-repairing ability. Conversely, the longer the crack healing time in the test results, the worse the self-repairing ability. The self-repairing ability test results are shown in Table 3. Therefore, the combined use of recycled oil and waste rubber powder can improve the self-repairing ability of asphalt mixture.

[0105] Table 3. Self-repair ability test results of Examples 1-5 and Comparative Examples 1-2

[0106] Test samples Crack healing time (h) Example 1 5 Example 2 4 Example 3 4.5 Example 4 5 Example 5 5 Comparative Example 1 12 Comparative Example 2 10

[0107] The seven groups of asphalt mixtures in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 were subjected to a material durability test. The test method was to perform 20 freeze-thaw cycle tests on the samples and measure the strength changes of the samples. The smaller the strength change value, the better the material durability. Conversely, the larger the strength change value, the worse the material durability. The material durability test results are shown in Table 4. Therefore, the use of SBS modified polymer emulsion can improve the anti-aging and wear resistance of asphalt mixtures, thereby increasing the service life and stability of the road surface.

[0108] Table 4. Test results of material durability of Examples 1-5 and Comparative Examples 1-2

[0109]

[0110]

[0111] The invention significantly reduces the heat absorption performance of asphalt mixture and improves water permeability and self-repairing ability by optimizing the formula and process. In addition, the improved production process improves the durability of the material, which has significant economic and social benefits.

[0112] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.

Claims

1. A warm mix regeneration agent, characterized in that: The invention comprises the following components by weight percentage: 10-20% of modified polymer emulsion, 2-5% of nano titanium dioxide, 5-10% of waste rubber powder, 10-20% of recycled oil and 45-60% of solvent.

2. The warm mix regeneration agent according to claim 1, characterized in that: The modified polymer emulsion is a styrene-butadiene-styrene (SBS) copolymer.

3. The warm mix regeneration agent according to claim 1, characterized in that: The particle size of the nano titanium dioxide is 20-50 nanometers.

4. The warm mix regeneration agent according to claim 1, characterized in that: The regenerated oil is a mixture of vegetable oil and mineral oil, and the ratio of the two is (4-7): (10-11).

5. An asphalt mixture, characterized in that: Contains 5-6wt% of the warm mix regeneration agent described in any one of claims 1 to 4.

6. The asphalt mixture according to claim 1, characterized in that: The raw materials include the following mass percentages: 80-90% of base asphalt, 5-6% of warm mix regeneration agent, and 3-5% of mineral material.

7. The asphalt mixture according to claim 5, characterized in that: The base asphalt is road petroleum asphalt.

8. The asphalt mixture according to claim 5, characterized in that: The mineral material is basalt or limestone aggregate.

9. The method for preparing asphalt mixture according to any one of claims 5 to 8, characterized in that: The steps include: S1: Raw material preparation: prepare the base asphalt, warm mix regeneration agent and mineral materials in proportion; S2: Preparation of warm mix regeneration agent, mixing the modified polymer emulsion, nano titanium dioxide, waste rubber powder and recycled oil in proportion; S3: Asphalt mixture preparation: add warm mix regeneration agent into base asphalt, heat to 140-160℃, and stir evenly; S4: Warm mix, adding mineral material to the heated asphalt mixture and mixing at 120-140°C; S5: Mixture shaping and compacting: pouring the mixture into a mold and compacting it; S6: Cooling and curing: cooling the formed mixture at room temperature and curing.

Citation Information

Patent Citations

  • Rubber asphalt open-graded drainage pavement mixture capable of absorbing automobile exhaust

    CN103332904A

  • Preparation method for synergistic asphalt-recycling agent

    CN106497097A

  • Warm-mix asphalt modifier and preparation method thereof

    CN108641384A

  • High weatherability composite modified asphalt for high-speed railway asphalt concrete waterproof sealing layer

    CN110791111A

  • Preparation method of asphalt mixture for low-temperature paved and high-weather-resistant drainage pavement

    CN111056770A

Cited By

  • Reclaimed oil bio-based plastic mixed rubber sole material and preparation method thereof

    CN119775787A

  • Airport pavement asphalt layer in-situ thermal regeneration and stepped reinforcement comprehensive construction method

    CN121407464A