Paper-cut engraving plate formula and manufacturing process thereof

By using poplar wood flour, wheat flour and other raw materials, combined with firing, filtration and refining processes, durable paper-cutting stereotypes are prepared, which solves the problem of paper-cutting stereotypes being susceptible to moths and significantly improves their durability.

CN118725587APending Publication Date: 2024-10-01JINGCONG (ANHUI) CULTURE COMM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410925339.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing paper-cut stereotypes are prone to moth problems when stored for a long time, which affects their service life.

Method used

It uses poplar wood flour, wheat flour, talc powder, cypress shell powder, elm bark powder, paraffin, mutton oil and butter as raw materials, prepares it according to a specific proportion, and prepares it through firing, filtering, refining and boiling processes. Produce durable paper cutting materials.

Benefits of technology

Significantly reduces the borer rate of paper-cut stereotypes and improves their durability, making the made stereotypes less susceptible to borers and more durable.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of paper-cut engraving plates, and particularly relates to a paper-cut engraving plate formula and a manufacturing process thereof.The paper-cut engraving plate formula comprises, by weight, 4-8 parts of poplar powder, 6-10 parts of wheat flour, 1-5 parts of talcum powder, 1-5 parts of cypress shell powder, 1-5 parts of elm bark powder, 1-5 parts of paraffin, 2-6 parts of mutton fat and 8-12 parts of beef tallow; the poplar powder, the wheat flour, the talcum powder, the cypress shell powder, the elm bark powder, the paraffin, the mutton fat and the beef tallow are selected as the raw materials, then the raw materials are matched according to a certain proportion, the moth rate of the paper-cut engraving plate can be greatly reduced, and then the durability of the paper-cut engraving plate can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paper-cutting stereotypes, in particular to a paper-cutting stereotype formula and a manufacturing process thereof. Background Art

[0002] Paper cutting is a kind of paper cutting, one of the traditional Chinese handicrafts. There are different styles of paper cutting works in folk all over the country. As early as the Han and Tang Dynasties, folk women had the fashion of using gold and silver foil and colored silk to cut square flowers and birds and paste them on their temples as decorations. Later, it gradually developed. During festivals, people cut various stories of flowers, plants, animals or characters with colored paper and pasted them on windows (called "window flowers") and door lintels (called "door signs") as decorations. They are also used as gift decorations or embroidery patterns. The tool for paper cutting is generally only a pair of small scissors; some professional artists use a special carving knife to carve, which is called paper cutting.

[0003] However, the existing paper-cutting stereotypes are prone to the phenomenon of termites during long-term placement, which will affect the service life of the paper-cutting stereotypes. Therefore, a paper-cutting stereotype formula and a manufacturing process thereof are invented. Summary of the invention

[0004] In view of the above and / or existing problems in a paper-cutting stereotype formulation and its production process, the present invention is proposed.

[0005] Therefore, the object of the present invention is to provide a paper-cutting plate formula and a production process thereof, which can solve the above-mentioned existing problems.

[0006] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0007] A paper-cutting plate formula comprises raw materials, wherein the raw materials include, by weight, 4-8 parts of poplar wood powder, 6-10 parts of wheat flour, 1-5 parts of talcum powder, 1-5 parts of cypress shell powder, 1-5 parts of elm bark powder, 1-5 parts of paraffin wax, 2-6 parts of sheep oil, and 8-12 parts of butter.

[0008] As a preferred embodiment of the paper-cutting plate formula described in the present invention, the ingredients in the raw materials include, by weight: 4 parts of poplar wood powder, 6 parts of wheat flour, 1 part of talcum powder, 1 part of cypress shell powder, 1 part of elm bark powder, 1 part of paraffin, 2 parts of mutton fat, and 8 parts of butter.

[0009] As a preferred embodiment of the paper-cutting plate formula described in the present invention, the ingredients in the raw materials include, by weight: 6 parts of poplar wood powder, 8 parts of wheat flour, 3 parts of talcum powder, 3 parts of cypress shell powder, 3 parts of elm bark powder, 3 parts of paraffin, 4 parts of mutton fat, and 10 parts of butter.

[0010] As a preferred embodiment of the paper-cutting plate formula described in the present invention, the ingredients in the raw materials include, by weight: 8 parts of poplar wood powder, 10 parts of wheat flour, 5 parts of talcum powder, 5 parts of cypress shell powder, 5 parts of elm bark powder, 5 parts of paraffin, 6 parts of mutton fat, and 12 parts of butter.

[0011] A process for making a paper-cutting plate comprises the following specific steps:

[0012] Step 1: placing poplar wood powder, talcum powder, cypress shell powder and elm bark powder in a blender according to a certain proportion and stirring and mixing them, and then burning the mixed poplar wood powder, talcum powder, cypress shell powder and elm bark powder to burn the poplar wood powder, talcum powder, cypress shell powder and elm bark powder into ash for later use;

[0013] Step 2: Cool the ash obtained in step 1 to a certain temperature, and then filter it with a filter to filter out impurities;

[0014] Step 3: Place the ash from step 2 in a blender, then place wheat flour in the blender and mix with the ash according to the proportion;

[0015] Step 4: Cut the mutton fat and beef tallow into pieces according to the proportion, and put them into the iron pot. Then, refine them with high heat first, and then refine them slowly with medium heat after refining for a while. After refining is completed, remove the oil residue;

[0016] Step 5: Put the paraffin into the refined oil pan according to the proportion and melt it;

[0017] Step 6: Place the ash powder mixed in step 3 in a melted oil pan and simmer over a low heat. During this process, use a spatula to stir the pan up and down until the ash powder and oil are integrated. At this point, the material for the paper-cutting plate can be prepared.

[0018] Step seven: Place the cooked paper-cutting plate material in the prepared plate container while it is still hot. During this process, not only should you move quickly, but you should also press it hard with a shovel, spreading it with the shovel while pressing to form a solid and flat putty block. At this point, you can get a durable paper-cutting plate that is resistant to moths.

[0019] As a preferred solution of the production process of a paper-cutting engraving plate described in the present invention, wherein: the mixing time in the step 1 is 6 min-10 min, and the mixing temperature is 40° C.-80° C.

[0020] As a preferred solution of the production process of a paper-cutting engraving plate described in the present invention, wherein: the cooling temperature of the ash in the step 2 is 20°C-24°C, and the filter diameter of the filter is 500μm-510μm.

[0021] As a preferred solution of the production process of the paper-cutting engraving plate described in the present invention, the mixing time in the step three is 6 min-10 min, and the mixing temperature is 30° C.-34° C.

[0022] As a preferred solution of the production process of the paper-cutting engraving plate described in the present invention, wherein: the high fire temperature in the step four is 180℃-220℃, the high fire refining time is 6min-10min, and the medium fire temperature is 60℃-80℃.

[0023] As a preferred solution of the process for making a paper-cutting engraving plate described in the present invention, the temperature of the warm fire in step six is ​​40°C-50°C.

[0024] Compared with existing technologies:

[0025] By selecting poplar wood powder, wheat flour, talcum powder, cypress shell powder, elm bark powder, paraffin, sheep oil and beef tallow as raw materials, and then mixing them according to a certain ratio, the insect rate of paper-cutting plates can be greatly reduced, thereby improving the durability of paper-cutting plates. DETAILED DESCRIPTION

[0026] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be described in further detail below.

[0027] Embodiment 1:

[0028] The invention provides a paper-cutting plate formula, comprising raw materials, wherein the raw materials include, by weight, 4 parts of poplar wood powder, 6 parts of wheat flour, 1 part of talcum powder, 1 part of cypress shell powder, 1 part of elm bark powder, 1 part of paraffin, 2 parts of sheep oil, and 8 parts of butter.

[0029] A process for making a paper-cutting plate comprises the following specific steps:

[0030] Step 1: Put poplar wood powder, talcum powder, cypress shell powder and elm bark powder in a blender according to a proportion and stir and mix them. The mixing time is 6 minutes and the mixing temperature is 40° C. Then, the mixed poplar wood powder, talcum powder, cypress shell powder and elm bark powder are burned to be able to burn the poplar wood powder, talcum powder, cypress shell powder and elm bark powder into ash for standby use;

[0031] Step 2: Cool the ash obtained in step 1 to a certain temperature (i.e., the cooling temperature of the ash is 20° C.), and then filter it with a filter to filter out impurities. The filter diameter of the filter is 500 μm.

[0032] Step 3: Place the ash in step 2 in a blender, then place wheat flour in a blender and mix with the ash according to the proportion, the mixing time is 6 minutes, and the mixing temperature is 30°C;

[0033] Step 4: Cut the mutton fat and beef tallow into pieces according to the proportion, and put them into an iron pot. Then, refine them with high heat first, and then refine them slowly with medium heat after refining for a period of time. After refining is completed, remove the oil residue. The high heat temperature is 180℃, the high heat refining time is 6 minutes, and the medium heat temperature is 60℃;

[0034] Step 5: Put the paraffin into the refined oil pan according to the proportion and melt it;

[0035] Step 6: Place the ash powder mixed in step 3 in a melted oil pan and simmer over a warm fire. During this process, use a spatula to stir the pan up and down until the ash powder and oil are integrated. At this point, the material for the paper-cutting plate can be prepared. The warm fire temperature is 40°C.

[0036] Step seven: Place the cooked paper-cutting plate material in the prepared plate container while it is still hot. During this process, not only should you move quickly, but you should also press it hard with a shovel, spreading it with the shovel while pressing to form a solid and flat putty block. At this point, you can get a durable paper-cutting plate that is resistant to moths.

[0037] Embodiment 2:

[0038] The invention provides a paper-cutting plate formula, comprising raw materials, wherein the raw materials include, by weight, 5 parts of poplar wood powder, 7 parts of wheat flour, 2 parts of talcum powder, 2 parts of cypress shell powder, 2 parts of elm bark powder, 2 parts of paraffin, 3 parts of sheep oil and 9 parts of butter.

[0039] A process for making a paper-cutting plate comprises the following specific steps:

[0040] Step 1: Put poplar wood powder, talcum powder, cypress shell powder and elm bark powder in a blender according to a proportion and stir and mix them. The mixing time is 7 minutes and the mixing temperature is 50° C. Then, the mixed poplar wood powder, talcum powder, cypress shell powder and elm bark powder are burned to be ash for standby use;

[0041] Step 2: Cool the ash obtained in step 1 to a certain temperature (i.e., the cooling temperature of the ash is 21° C.), and then filter it with a filter to filter out impurities. The filter diameter of the filter is 502.5 μm.

[0042] Step 3: Place the ash in step 2 in a blender, then place wheat flour in a blender and mix with the ash according to the proportion, the mixing time is 7 minutes, and the mixing temperature is 31°C;

[0043] Step 4: Cut the mutton fat and beef tallow into pieces according to the proportion, and put them into an iron pot. Then, refine them with high heat first, and then refine them slowly with medium heat after refining for a period of time. After refining is completed, remove the oil residue. The high heat temperature is 190℃, the high heat refining time is 7 minutes, and the medium heat temperature is 65℃;

[0044] Step 5: Put the paraffin into the refined oil pan according to the proportion and melt it;

[0045] Step 6: Place the ash powder mixed in step 3 in a melted oil pan and simmer over a warm fire. During this process, use a spatula to stir the pan up and down until the ash powder and oil are integrated. At this point, the material for the paper-cutting plate can be prepared. The warm fire temperature is 42.5°C.

[0046] Step seven: Place the cooked paper-cutting plate material in the prepared plate container while it is still hot. During this process, not only should you move quickly, but you should also press it hard with a shovel, spreading it with the shovel while pressing to form a solid and flat putty block. At this point, you can get a durable paper-cutting plate that is resistant to moths.

[0047] Embodiment 3:

[0048] The invention provides a paper-cutting plate formula, comprising raw materials, wherein the raw materials include, by weight, 6 parts of poplar wood powder, 8 parts of wheat flour, 3 parts of talcum powder, 3 parts of cypress shell powder, 3 parts of elm bark powder, 3 parts of paraffin, 4 parts of sheep oil, and 10 parts of butter.

[0049] A process for making a paper-cutting plate comprises the following specific steps:

[0050] Step 1: Put poplar wood powder, talcum powder, cypress shell powder and elm bark powder in a blender according to a certain proportion and stir and mix them. The mixing time is 8 minutes and the mixing temperature is 60° C. Then, the mixed poplar wood powder, talcum powder, cypress shell powder and elm bark powder are burned to be ash for later use;

[0051] Step 2: Cool the ash obtained in step 1 to a certain temperature (i.e., the cooling temperature of the ash is 22° C.), and then filter it with a filter to filter out impurities. The filter diameter of the filter is 505 μm.

[0052] Step 3: Place the ash in step 2 in a blender, then place wheat flour in a blender and mix with the ash according to the proportion, the mixing time is 8 minutes, and the mixing temperature is 32°C;

[0053] Step 4: Cut the mutton fat and beef tallow into pieces according to the proportion, and put them into an iron pot. Then, refine them with high heat first, and then refine them slowly with medium heat after refining for a period of time. After refining is completed, remove the oil residue. The high heat temperature is 200℃, the high heat refining time is 8 minutes, and the medium heat temperature is 70℃;

[0054] Step 5: Put the paraffin into the refined oil pan according to the proportion and melt it;

[0055] Step 6: Place the ash powder mixed in step 3 in a melted oil pan and simmer over a warm fire. During this process, use a spatula to stir the pan up and down until the ash powder and oil are integrated. At this point, the material for the paper-cutting plate can be prepared. The warm fire temperature is 45°C.

[0056] Step seven: Place the cooked paper-cutting plate material in the prepared plate container while it is still hot. During this process, not only should you move quickly, but you should also press it hard with a shovel, spreading it with the shovel while pressing to form a solid and flat putty block. At this point, you can get a durable paper-cutting plate that is resistant to moths.

[0057] Embodiment 4:

[0058] The invention provides a paper-cutting plate formula, comprising raw materials, wherein the raw materials include, by weight, 7 parts of poplar wood powder, 9 parts of wheat flour, 4 parts of talcum powder, 4 parts of cypress shell powder, 4 parts of elm bark powder, 4 parts of paraffin, 5 parts of sheep oil, and 11 parts of butter.

[0059] A process for making a paper-cutting plate comprises the following specific steps:

[0060] Step 1: Put poplar wood powder, talcum powder, cypress shell powder and elm bark powder in a blender according to a proportion and stir and mix them. The mixing time is 9 minutes and the mixing temperature is 70° C. Then, the mixed poplar wood powder, talcum powder, cypress shell powder and elm bark powder are burned to be able to burn the poplar wood powder, talcum powder, cypress shell powder and elm bark powder into ash for standby use;

[0061] Step 2: Cool the ash obtained in step 1 to a certain temperature (i.e., the cooling temperature of the ash is 23° C.), and then filter it with a filter to filter out impurities. The filter diameter of the filter is 507.5 μm.

[0062] Step 3: Place the ash in step 2 in a blender, then place wheat flour in a blender and mix with the ash according to the proportion, the mixing time is 9 minutes, and the mixing temperature is 33°C;

[0063] Step 4: Cut the mutton fat and beef tallow into pieces according to the proportion, and put them into an iron pot. Then, refine them with high heat first, and then refine them slowly with medium heat after refining for a period of time. After refining, remove the oil residue. The high heat temperature is 210℃, the high heat refining time is 9 minutes, and the medium heat temperature is 75℃;

[0064] Step 5: Put the paraffin into the refined oil pan according to the proportion and melt it;

[0065] Step 6: Place the ash powder mixed in step 3 in a melted oil pan and simmer over a warm fire. During this process, use a spatula to stir the pan up and down until the ash powder and oil are integrated. At this point, the material for the paper-cutting plate can be prepared. The warm fire temperature is 47.5°C.

[0066] Step seven: Place the cooked paper-cutting plate material in the prepared plate container while it is still hot. During this process, not only should you move quickly, but you should also press it hard with a shovel, spreading it with the shovel while pressing to form a solid and flat putty block. At this point, you can get a durable paper-cutting plate that is resistant to moths.

[0067] Embodiment 5:

[0068] The invention provides a paper-cutting plate formula, comprising raw materials, wherein the raw materials include, by weight, 8 parts of poplar wood powder, 10 parts of wheat flour, 5 parts of talcum powder, 5 parts of cypress shell powder, 5 parts of elm bark powder, 5 parts of paraffin, 6 parts of sheep oil, and 12 parts of butter.

[0069] A process for making a paper-cutting plate comprises the following specific steps:

[0070] Step 1: Put poplar wood powder, talcum powder, cypress shell powder and elm bark powder in a blender according to a proportion and stir and mix them. The mixing time is 10 minutes and the mixing temperature is 80° C. Then, the mixed poplar wood powder, talcum powder, cypress shell powder and elm bark powder are burned to be ash for standby use;

[0071] Step 2: Cool the ash obtained in step 1 to a certain temperature (i.e., the cooling temperature of the ash is 24° C.), and then filter it with a filter to filter out impurities. The filter diameter of the filter is 510 μm.

[0072] Step 3: Place the ash in step 2 in a blender, then place wheat flour in a blender and mix with the ash according to the proportion, the mixing time is 10 minutes, and the mixing temperature is 34°C;

[0073] Step 4: Cut the mutton fat and beef tallow into pieces according to the proportion, and put them into an iron pot. Then, refine them with high heat first, and then refine them slowly with medium heat after refining for a period of time. After refining is completed, remove the oil residue. The high heat temperature is 220℃, and the high heat refining time is 10 minutes, and the medium heat temperature is 80℃;

[0074] Step 5: Put the paraffin into the refined oil pan according to the proportion and melt it;

[0075] Step 6: Place the ash powder mixed in step 3 in a melted oil pan and simmer over a warm fire. During this process, use a spatula to stir the pan up and down until the ash powder and oil are integrated. At this point, the material for the paper-cutting plate can be prepared. The warm fire temperature is 50°C.

[0076] Step seven: Place the cooked paper-cutting plate material in the prepared plate container while it is still hot. During this process, not only should you move quickly, but you should also press it hard with a shovel, spreading it with the shovel while pressing to form a solid and flat putty block. At this point, you can get a durable paper-cutting plate that is resistant to moths.

[0077] The paper-cutting stereotypes prepared in the above Examples 1-5 were compared to obtain the following data:

[0078] Example 1 Example 2 Example 3 Example 4 Example 5 Borer rate 2.2% 1.6% 1.1% 2.3% 1.3%

[0079] It can be seen from the above table that the paper-cutting boards prepared in Examples 1-5 have better performance in terms of insect borer rate. However, the different proportions of poplar wood powder, wheat flour, talcum powder, cypress shell powder, elm bark powder, paraffin, sheep oil and butter result in different effects on the insect borer rate of the paper-cutting boards. After use, Example 3 has the best effect.

[0080] Although the present invention has been described above with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no structural conflict, the various features in the embodiments disclosed in the present invention may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A paper-cutting plate formula, comprising raw materials, characterized in that: The raw materials include, by weight: 4-8 parts of poplar wood powder, 6-10 parts of wheat flour, 1-5 parts of talcum powder, 1-5 parts of cypress shell powder, 1-5 parts of elm bark powder, 1-5 parts of paraffin, 2-6 parts of sheep oil, and 8-12 parts of butter.

2. A paper cutting plate formula according to claim 1, characterized in that: The ingredients in the raw materials include, by weight: 4 parts of poplar wood powder, 6 parts of wheat flour, 1 part of talcum powder, 1 part of cypress shell powder, 1 part of elm bark powder, 1 part of paraffin, 2 parts of sheep oil, and 8 parts of butter.

3. A paper cutting plate formula according to claim 1, characterized in that: The ingredients in the raw materials include, by weight: 6 parts of poplar wood powder, 8 parts of wheat flour, 3 parts of talcum powder, 3 parts of cypress shell powder, 3 parts of elm bark powder, 3 parts of paraffin, 4 parts of sheep oil, and 10 parts of butter.

4. A paper cutting plate formula according to claim 1, characterized in that: The ingredients in the raw materials include, by weight: 8 parts of poplar wood powder, 10 parts of wheat flour, 5 parts of talcum powder, 5 parts of cypress shell powder, 5 parts of elm bark powder, 5 parts of paraffin, 6 parts of sheep oil, and 12 parts of butter.

5. A process for making a paper-cutting plate, characterized in that: The specific steps are as follows: Step 1: placing poplar wood powder, talcum powder, cypress shell powder and elm bark powder in a blender according to a certain proportion and stirring and mixing them, and then burning the mixed poplar wood powder, talcum powder, cypress shell powder and elm bark powder to burn the poplar wood powder, talcum powder, cypress shell powder and elm bark powder into ash for later use; Step 2: Cool the ash obtained in step 1 to a certain temperature, and then filter it with a filter to filter out impurities; Step 3: Place the ash from step 2 in a blender, then place wheat flour in the blender and mix with the ash according to the proportion; Step 4: Cut the mutton fat and beef tallow into pieces according to the proportion, and put them into the iron pot. Then, refine them with high heat first, and then refine them slowly with medium heat after refining for a while. After refining is completed, remove the oil residue; Step 5: Put the paraffin into the refined oil pan according to the proportion and melt it; Step 6: Place the ash powder mixed in step 3 in a melted oil pan and simmer over a low heat. During this process, use a spatula to stir the pan up and down until the ash powder and oil are integrated. At this point, the material for the paper-cutting plate can be prepared. Step seven: Place the cooked paper-cutting plate material in the prepared plate container while it is still hot. During this process, not only should you move quickly, but you should also press it hard with a shovel, spreading it with the shovel while pressing to form a solid and flat putty block. At this point, you can get a durable paper-cutting plate that is resistant to moths.

6. The process for making a paper-cutting plate according to claim 5, characterized in that: In the step 1, the mixing time is 6 min-10 min, and the mixing temperature is 40° C.-80° C.

7. The process for making a paper-cutting plate according to claim 5, characterized in that: In the step 2, the cooling temperature of the ash is 20° C.-24° C., and the filter diameter of the filter is 500 μm-510 μm.

8. The process for making a paper-cutting plate according to claim 5, characterized in that: In the step 3, the mixing time is 6 min-10 min, and the mixing temperature is 30° C.-34° C.

9. The process for making a paper-cutting plate according to claim 5, characterized in that: In step 4, the high-fire temperature is 180°C-220°C, the high-fire refining time is 6min-10min, and the medium-fire temperature is 60°C-80°C.

10. The process for making a paper-cutting plate according to claim 5, characterized in that: The temperature of the medium heat in step 6 is 40°C-50°C.