Liquid crystal polymer composition as well as preparation method and application thereof
By selecting the appropriate melting point difference between liquid crystal polymer resin and fiber and the density of hollow glass beads, a liquid crystal polymer composition with low thermal conductivity and high tensile strength is prepared, which solves the problem of performance matching of liquid crystal polymer materials in heated parts and satisfies Meets the application requirements of high strength and low thermal conductivity.
Patent Information
- Application Number
- CN202310314158.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
Liquid crystal polymer materials have difficulty balancing low thermal conductivity and high tensile strength, which limits their application in heated parts of office equipment and small household appliances.
By rationally selecting the melting point difference between the liquid crystal polymer resin and the liquid crystal polymer fiber, adding hollow glass beads of a specific density, and adjusting the strength and component ratio of the liquid crystal polymer fiber, a thermal conductivity coefficient below 0.3W/M/K was prepared. , a liquid crystal polymer composition with a tensile strength greater than 50MPa.
It achieves material performance matching in scenarios with high strength and low thermal conductivity requirements, meets the use requirements of components, and demonstrates the impact of different component ratios on performance through specific examples.
Smart Images

Figure BDA0004149623940000051 
Figure BDA0004149623940000052 
Figure BDA0004149623940000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of engineering plastics, and more specifically, to a liquid crystal polymer composition and a preparation method and application thereof. Background Art
[0002] Liquid crystal polymer (TLCP) can be used in office equipment (such as printers, projectors, etc.) and small household appliances due to its high heat resistance, high dimensional stability, high strength and other characteristics. The structural parts, such as printer fixing unit, induction cooker temperature sensor, microwave oven door frame insulation belt, etc.; however, these structural parts often require the material to have low thermal conductivity, while the molecular chain of liquid crystal polymer is arranged regularly and densely, and it is a high crystallinity material with a high thermal conductivity. In order to obtain liquid crystal polymer materials with lower thermal conductivity, the thermal conductivity can be reduced by adding hollow glass microspheres. For example, the Chinese patent named "A Liquid Crystal Polymer Composition and Its Application" adds hollow glass microspheres, which can reduce the thermal conductivity of the material, but the addition of hollow glass microspheres will greatly reduce the tensile strength of the material, which still limits the application scenarios of liquid crystal polymers.
[0003] To this end, it is necessary to solve the problem that the current liquid crystal polymer materials have low thermal conductivity and high strength and are difficult to achieve at the same time. Summary of the invention
[0004] The primary purpose of the present invention is to overcome the problem that the low thermal conductivity and high strength of the current liquid crystal polymer materials are difficult to achieve at the same time, and to provide a liquid crystal polymer composition. The thermal conductivity of the liquid crystal polymer composition is below 0.3W / M / K, and the tensile strength is greater than 50MPa, which meets the use requirements of the scene where the components have high strength and low thermal conductivity requirements.
[0005] A further object of the present invention is to provide a method for preparing the above liquid crystal polymer composition.
[0006] A further object of the present invention is to provide use of the liquid crystal polymer composition in preparing a heat receiving component of an OA device or a heat receiving component of a small household appliance.
[0007] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0008] A liquid crystal polymer composition comprises the following components in parts by weight:
[0009] 100 parts of liquid crystal polymer resin, 10-50 parts of liquid crystal polymer fibers, and 10-50 parts of hollow glass microspheres;
[0010] The melting point T of the liquid crystal polymer resin m1 The melting point T of the liquid crystal polymer fiber m2 The difference (T m2 -Tm1 )≥30℃; the strength of the liquid crystal polymer fiber is ≥5cN / dtex; the density of the hollow glass microsphere is ≤0.6g / cm 3 ;
[0011] In the present invention, the liquid crystal polymer resin is a thermotropic liquid crystal polymer resin, and the liquid crystal polymer fiber is a thermotropic liquid crystal polymer fiber.
[0012] The inventors of the present invention have discovered through multiple studies that by selecting liquid crystal polymer resins and liquid crystal polymer fibers with specific melting point differences and hollow glass microbeads with specific density, and further regulating the strength of the liquid crystal polymer fibers and the amount of each component, a liquid crystal polymer composition with high strength and low thermal conductivity can be obtained. The thermal conductivity of the liquid crystal polymer composition is below 0.3W / M / K, and the tensile strength is greater than 50MPa, which meets the use requirements of scenarios where components require high strength and low thermal conductivity.
[0013] The strength of the liquid crystal polymer fiber of the present invention can be measured according to ISO 2062-2009 standard.
[0014] The density of the hollow glass microspheres of the present invention refers to the true density, which can be measured according to the gas displacement method of standard ASTM D5965-02.
[0015] The liquid crystal polymer fiber of the present invention refers to a liquid crystal polymer resin in a fibrous form in a liquid crystal polymer composition, with a length of 2 to 4 mm and a single fiber diameter of 10 to 60 dtex; the liquid crystal polymer fiber can be prepared by the following method: m2 The liquid crystal polymer resin is melted and plasticized, extruded through a spinneret, and cut to obtain the liquid crystal polymer fiber.
[0016] Preferably, the liquid crystal polymer composition comprises the following components in parts by weight: 100 parts of liquid crystal polymer resin, 15 to 45 parts of liquid crystal polymer fibers, and 15 to 45 parts of hollow glass microspheres.
[0017] Preferably, the melting point of the liquid crystal polymer resin is m1 The melting point T of the liquid crystal polymer fiber m2 The difference (T m2 -T m1 )≥32℃.
[0018] More preferably, the melting point of the liquid crystal polymer resin is m1 The melting point T of the liquid crystal polymer fiber m2 The difference (T m2 -T m1 ) is 58~90℃.
[0019] When the melting point difference is 58-90° C., the obtained liquid crystal polymer composition has lower thermal conductivity and higher tensile strength.
[0020] Preferably, the strength of the liquid crystal polymer fiber is 5.2-9.8 cN / dtex.
[0021] The liquid crystal polymer fiber within this strength range can enable the liquid crystal polymer composition to have a higher tensile strength while maintaining a low thermal conductivity.
[0022] Preferably, the density of the hollow glass microspheres is 0.50-0.55 g / cm 3 .
[0023] When the density of the hollow glass microspheres is within this range, the liquid crystal polymer composition can have a lower thermal conductivity.
[0024] Preferably, the liquid crystal polymer composition further comprises 0.1 to 3 parts of other auxiliary agents.
[0025] More preferably, the other auxiliary agent is at least one of an antioxidant or a lubricant.
[0026] Optionally, the antioxidant is selected from one or more of phenols, amines and sulfurs.
[0027] Optionally, the lubricant is selected from one or more of fluorine-containing polymers, linear low-density polyethylene (LLDPE), silicone oil, stearic acid metal salts, stearic acid alkyl esters, montanic acid metal salts, montanic acid ester wax or polyethylene wax.
[0028] The method for preparing the above-mentioned liquid crystal polymer composition comprises the following steps:
[0029] The components are mixed uniformly, melted, extruded and granulated to obtain the liquid crystal polymer composition; the melting temperature is T m1 ±5℃.
[0030] The use of the above liquid crystal polymer composition or the liquid crystal polymer composition prepared by the above preparation method in preparing heat-receiving parts of OA equipment or heat-receiving parts of small household appliances also falls within the protection scope of the present invention.
[0031] Preferably, the OA equipment is a printer or a projector, and the small household appliance is an induction cooker or a microwave oven.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The thermal conductivity of the liquid crystal polymer composition of the present invention is below 0.3 W / M / K, and the tensile strength is greater than 50 MPa, which meets the use requirements of the scene with high strength and low thermal conductivity requirements for components. DETAILED DESCRIPTION
[0034] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.
[0035] Some of the reagents selected in the embodiments and comparative examples of the present invention are described as follows:
[0036] Liquid crystal polymer resin 1#: Zhuhai Wantong Special Engineering Plastics, Vicryst R8000, T m1 The temperature is 280°C and the melt viscosity is 25 Pa.s;
[0037] Liquid crystal polymer resin 2#: Zhuhai Wantong Special Engineering Plastics, Vicryst R8500-A, T m1 The temperature is 338°C and the melt viscosity is 25 Pa.s;
[0038] Liquid crystal polymer resin 3#: Zhuhai Wantong Special Engineering Plastics, Vicryst R800, T m1 The temperature is 355°C and the melt viscosity is 25 Pa.s;
[0039] Liquid crystal polymer resin 4#: Zhuhai Wantong Special Engineering Plastics, Vicryst R8200, T m1 The temperature is 370°C and the melt viscosity is 25 Pa.s;
[0040] Liquid crystal polymer resin 5#: Zhuhai Wantong Special Engineering Plastics, Vicryst R8500-B, T m1 The temperature is 338°C and the melt viscosity is 35 Pa.s;
[0041] Liquid crystal polymer resin 6#: Zhuhai Wantong Special Engineering Plastics, Vicryst R8500-C, T m1 The temperature is 338°C and the melt viscosity is 20Pa.s;
[0042] Liquid crystal polymer resin 7#: Zhuhai Wantong Special Engineering Plastics, Vicryst R8500-D, T m1 The temperature is 338°C and the melt viscosity is 15 Pa.s;
[0043] Liquid crystal polymer resin 8#: Zhuhai Wantong Special Engineering Plastics, Vicryst R8500-E, T m1 The temperature is 338°C and the melt viscosity is 10Pa.s;
[0044] Liquid crystal polymer fibers 1 to 8#, homemade, were prepared by the following method:m1 Liquid crystal polymer resin (liquid crystal polymer tree 1-8#) is used as raw material, and then the raw material is added to a single screw extruder for melting and plasticization, and then extruded through a porous spinneret. After the melt leaves the spinneret die, it is guided by a traction roller and pulled to a cutting machine by a suction gun. The fiber is cut into a length of 3 mm and a single filament diameter of 10-60 dtex to obtain a melting point of T m2 Liquid crystal polymer fiber. The melting point of liquid crystal polymer is mainly determined by the different monomer compositions. The melting point of liquid crystal polymer fiber does not change when liquid crystal polymer resin is prepared into liquid crystal polymer fiber, so the melting point of liquid crystal polymer fiber is consistent with the melting point of its raw material (liquid crystal polymer resin).
[0045] For liquid crystal polymer resins with the same melting point, polymer fibers with different strengths can be obtained by adjusting the melt viscosity, i.e., molecular weight, of the liquid crystal polymer. Specifically, the reaction that occurs during the preparation of the liquid crystal polymer is a polycondensation reaction. The longer the reaction time, the higher the viscosity, the longer the molecular chain, i.e., the larger the molecular weight, and the higher the strength of the liquid crystal polymer fiber obtained as a raw material; therefore, by controlling the time of its polycondensation reaction, liquid crystal polymers with different viscosities can be easily obtained, thereby obtaining liquid crystal polymer fibers with different strengths. The raw material supplier adjusts the polycondensation reaction time of the liquid crystal polymer resin R8500 to control its melt viscosity, and obtains liquid crystal polymer resins with different melt viscosities. Then, by processing the liquid crystal polymer resins with different melt viscosities, liquid crystal polymer fibers with the same melting point but different strengths are obtained, i.e., liquid crystal polymer fibers 2#, 5# to 8#.
[0046] For the melt viscosity test, a capillary rheometer was used according to ISO 11443 standard at T m1 +15℃、1000s -1 Measured under conditions.
[0047] Liquid crystal polymer fiber 1#: the raw material is liquid crystal polymer resin 1#, T m2 The temperature is 280℃ and the strength is 9.8cN / dtex;
[0048] Liquid crystal polymer fiber 2#: the raw material is liquid crystal polymer resin 2#, T m2 The temperature is 338℃ and the strength is 8.4cN / dtex;
[0049] Liquid crystal polymer fiber 3#: the raw material is liquid crystal polymer resin 3#, T m2 355℃, strength 5.2cN / dtex;
[0050] Liquid crystal polymer fiber 4#: the raw material is liquid crystal polymer resin 4#, T m2 The temperature is 370℃ and the strength is 6.3cN / dtex;
[0051] Liquid crystal polymer fiber 5#: the raw material is liquid crystal polymer resin 5#, T m2 338℃, strength 9.6cN / dtex;
[0052] Liquid crystal polymer fiber 6#: the raw material is liquid crystal polymer resin 6#, T m2 The temperature is 338℃ and the strength is 6.1cN / dtex;
[0053] Liquid crystal polymer fiber 7#: the raw material is liquid crystal polymer resin 7#, T m2 338℃, strength 5.0cN / dtex;
[0054] Liquid crystal polymer fiber 8#: the raw material is liquid crystal polymer resin 8#, T m2 338℃, strength 4.3cN / dtex;
[0055] Hollow glass microsphere 1#: Zhengzhou Saint-Laite hollow microsphere new material, HL50, density 0.5g / cm 3 ;
[0056] Hollow glass microsphere 2#: Zhengzhou Saint-Laite hollow microsphere new material, HL55, density 0.55g / cm 3 ;
[0057] Hollow glass microsphere 3#: Zhengzhou Saint-Laite hollow microsphere new material, HL60S, density 0.6g / cm 3 ;
[0058] Hollow glass microsphere 4#: Zhengzhou Saint-Laite hollow microsphere new material, HS70, density 0.7g / cm 3 ;
[0059] Inorganic fiber: Owens Corning, model 923, average diameter 10 μm, initial average length 3 mm;
[0060] Other additives: lubricant, linear low-density polyethylene, commercially available;
[0061] Unless otherwise specified, the components (such as other auxiliary agents) selected in the parallel examples and comparative examples are all the same commercially available products.
[0062] The properties of the liquid crystal polymer compositions provided in the embodiments and comparative examples of the present invention were measured according to the following test methods:
[0063] Tensile strength: Prepare tensile specimens with a size of 110mm*10mm*4mm and test them according to ISO 527-2019 standard;
[0064] Thermal conductivity: laser flash method, prepare 100mm*100mm*3mm sample, and test according to GB / T22588-2008 standard;
[0065] The preparation process of the liquid crystal polymer composition of each embodiment of the present invention and each comparative example is as follows: the components are mixed uniformly, m1 The liquid crystal polymer composition is melted, extruded and granulated at +5°C.
[0066] Examples 1 to 19
[0067] Examples 1 to 19 provide a series of liquid crystal polymer compositions, whose formulations are shown in Table 1 and Table 2.
[0068] Table 1 Formulas of Examples 1 to 11 (parts by weight)
[0069]
[0070] Table 2 Formulations of Examples 12 to 19 (parts by weight)
[0071]
[0072]
[0073] Comparative Example 1
[0074] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that the liquid crystal polymer fiber 2# is replaced by the liquid crystal polymer fiber 1#.
[0075] Comparative Example 2
[0076] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that liquid crystal polymer fiber 2# is replaced by liquid crystal polymer fiber 8#.
[0077] Comparative Example 3
[0078] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that liquid crystal polymer fiber 2# is replaced by liquid crystal polymer fiber 3#, and liquid crystal polymer resin 1# is replaced by liquid crystal polymer resin 2#.
[0079] Comparative Example 4
[0080] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that the amount of liquid crystal polymer fiber 2# used is 60 parts by weight.
[0081] Comparative Example 5
[0082] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that the amount of liquid crystal polymer fiber 2# used is 5 parts by weight.
[0083] Comparative Example 6
[0084] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that hollow glass microspheres 1# are replaced with hollow glass microspheres 4#.
[0085] Comparative Example 7
[0086] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that the amount of hollow glass microspheres 1# used is 60 parts by weight.
[0087] Comparative Example 8
[0088] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that the amount of hollow glass microspheres 1# used is 5 parts by weight.
[0089] Comparative Example 9
[0090] This comparative example provides a liquid crystal polymer composition, the formula of which is different from that of Example 1 in that the liquid crystal polymer fiber 2# is replaced by inorganic fiber.
[0091] The properties of the liquid crystal polymer compositions of the embodiments and comparative examples were measured according to the above-mentioned test methods. The test results are shown in Table 3.
[0092] Table 3 Performance test results of the liquid crystal polymer compositions of various embodiments and comparative examples
[0093]
[0094]
[0095] From Table 3, we can see that:
[0096] The tensile strength of the liquid crystal polymer compositions of Examples 1 to 19 is higher than 50 MPa, and the thermal conductivity is lower than 0.3 W / M / K, indicating that the liquid crystal polymer compositions of the present invention have low thermal conductivity and high tensile strength, meeting the use requirements of scenes with high strength and low thermal conductivity requirements for components. Among them, it can be seen from Examples 6, 7, 1, 8 and 9 that with the increase in the amount of liquid crystal polymer fiber, the tensile strength of the liquid crystal polymer composition first increases and then decreases. This is because when there are more liquid crystal polymer fibers (Examples 8 and 9), the dispersion of the liquid crystal polymer fibers decreases to a certain extent, resulting in a decrease in the tensile strength of the liquid crystal polymer composition; in addition, the decrease in the dispersion of the liquid crystal polymer fibers will also cause the liquid crystal polymer composition to have certain microscopic pores, resulting in a slight decrease in thermal conductivity (for example, the thermal conductivity of Example 9 is slightly decreased relative to Example 8).
[0097] In Comparative Example 1, liquid crystal polymer fiber 1# was added, and the melting point difference between liquid crystal polymer fiber 1# and liquid crystal polymer resin 1# was less than 30°C, resulting in the final liquid crystal polymer composition having too low tensile strength; in Comparative Example 2, liquid crystal polymer fiber 8# was added, and the strength of liquid crystal polymer fiber 8# was relatively low, resulting in the final liquid crystal polymer composition having too low tensile strength; in Comparative Example 3, liquid crystal polymer fiber 3# and liquid crystal polymer resin 2# were added, and the melting point difference between the two was 17°C, resulting in the final liquid crystal polymer composition having too low tensile strength; in Comparative Example 4, too much liquid crystal polymer fiber 2# was added, and the dispersibility was poor, resulting in the final liquid crystal polymer composition having too low tensile strength. The tensile strength of the liquid crystal polymer composition is too low, and too little liquid crystal polymer fiber 2# is added in comparative example 5, resulting in that the tensile strength of the liquid crystal polymer composition obtained is also too low; hollow glass microspheres 4# are added in comparative example 6, and since the density of hollow glass microspheres 4# is too large, the thermal conductivity of the liquid crystal polymer composition obtained is too high; too much hollow glass microspheres 1# are added in comparative example 7, resulting in that the tensile strength of the liquid crystal polymer composition obtained is too low, and too little hollow glass microspheres 1# are added in comparative example 8, resulting in that the thermal conductivity of the liquid crystal polymer composition obtained is too high; inorganic fibers are added in comparative example 9, resulting in that the thermal conductivity of the liquid crystal polymer composition obtained is too high.
[0098] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A liquid crystal polymer composition, characterized in that The composition comprises the following components in parts by weight: 100 parts of liquid crystal polymer resin, 10-50 parts of liquid crystal polymer fibers, and 10-50 parts of hollow glass microspheres; The melting point T of the liquid crystal polymer resin m1 The melting point T of the liquid crystal polymer fiber m2 The difference (T m2 -T m1 )≥30℃; the strength of the liquid crystal polymer fiber is ≥5cN / dtex; the density of the hollow glass microsphere is ≤0.6g / cm 3 .
2. The liquid crystal polymer composition according to claim 1, characterized in that: The liquid crystal polymer combination comprises the following components in parts by weight: 100 parts of liquid crystal polymer resin, 15 to 45 parts of liquid crystal polymer fibers, and 15 to 45 parts of hollow glass microspheres.
3. The liquid crystal polymer composition according to claim 1, characterized in that: The melting point T of the liquid crystal polymer resin m1 The melting point T of the liquid crystal polymer fiber m2 The difference (T m2 -T m1 ) is ≥32℃.
4. The liquid crystal polymer composition according to claim 3, characterized in that: The melting point T of the liquid crystal polymer resin m1 The melting point T of the liquid crystal polymer fiber m2 The difference (T m2 -T m1 ) is 58~90℃.
5. The liquid crystal polymer composition according to claim 1, characterized in that: The strength of the liquid crystal polymer fiber is 5.2-9.8 cN / dtex.
6. The liquid crystal polymer composition according to claim 1, characterized in that: The density of the hollow glass microspheres is 0.50-0.55 g / cm 3 .
7. The liquid crystal polymer composition according to claim 1, characterized in that: The liquid crystal polymer composition further comprises 0.1 to 3 parts of other auxiliary agents.
8. The liquid crystal polymer composition according to claim 1, characterized in that: The other auxiliary agent is at least one of an antioxidant and a lubricant.
9. The method for preparing a liquid crystal polymer composition according to any one of claims 1 to 8, characterized in that: The steps include: The components are mixed uniformly, melted, extruded and granulated to obtain the liquid crystal polymer composition; the melting temperature is T m1 +5℃.
10. Use of the liquid crystal polymer composition according to any one of claims 1 to 8 or the liquid crystal polymer composition prepared by the preparation method according to claim 9 in preparing heat-receiving parts of OA equipment or heat-receiving parts of small household appliances.