Steel wire rope lubricating grease and preparation method thereof
By optimizing the formula and cooling process of the wire rope grease, we have solved the problems of high cost and complex process in the existing technology, and prepared wire rope grease suitable for different application scenarios, achieving the performance of not slipping at high temperatures and not brittle at low temperatures, meeting the requirements production and maintenance needs.
Patent Information
- Application Number
- CN202410787013.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
AI Technical Summary
Existing wire rope greases are difficult to meet the diverse protection needs of steel wire ropes during production and use due to high costs and complex processes. In particular, they lack the properties of non-slip at high temperatures and non-brittleness at low temperatures in harsh environments.
Using the formula of hot mix asphalt regenerant, naphthenic oil, thickener, pour point depressant and rust inhibitor, and by optimizing the formula composition and cooling process, wire rope greases in different finished product states are prepared to improve film-forming performance and Low temperature performance, reducing costs and simplifying processes.
The wire rope grease used in the production and maintenance process has excellent wear resistance, anti-rust and lubrication properties, meeting the needs of different application scenarios, while reducing raw material costs and process complexity.
Smart Images

Figure CN118725939A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of protective agents, and in particular relates to a steel wire rope grease and a preparation method thereof. Background Art
[0002] Wire rope is an indispensable component of modern large-scale engineering equipment, elevators, bridges, etc. It can be said that the normal operation of these equipment depends largely on the wire rope. The wire rope is a product made of core rope and strand rope twisted together by external force. The core rope is mainly a fiber core or steel core, and the strand rope is 4-8 strands, which are a structure of multiple steel wires twisted together. During its production process, the core rope and the strand rope will produce friction and wear due to the twisting action. During its use, the wire rope will be subjected to great tension, which will also cause serious wear between the strands. Therefore, the wire rope needs lubrication and protection both during the production process and during use.
[0003] With the development of economy and the deepening of industrialization, many large-scale engineering equipment are operated in very harsh environments, such as offshore platforms, mines, polar regions, etc., which puts forward high requirements on the protection and maintenance of wire ropes, such as rust prevention, wear resistance, no slipping at high temperature, no brittle cracking at low temperature, etc. If the existing wire rope grease wants to have better performance, either the raw material cost is high or the process is complicated, and it can only be used alone in the production or operation and maintenance process.
[0004] Therefore, in view of the above technical problems, it is necessary to provide a wire rope grease and a preparation method.
[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0006] The purpose of the present invention is to provide a steel wire rope grease and a preparation method, which can greatly reduce costs and simplify processes. It also realizes a steel wire rope grease that can adopt different cooling processes to obtain different finished product states, so that it can meet the needs of different application scenarios, such as being used at the production end and also being used in the later operation and maintenance process.
[0007] In order to achieve the above-mentioned purpose, a technical solution provided by a specific embodiment of the present invention is as follows: the raw materials of the wire rope grease include, by weight: asphalt regeneration agent for hot mix: 60-85 parts; cycloalkyl oil: 10-30 parts; thickener: 4-20 parts; pour point depressant: 1-5 parts; rust inhibitor: 0-1 part.
[0008] In one or more embodiments of the present invention, the hot mix asphalt rejuvenator is selected from: Iranian RA5 hot mix asphalt rejuvenator (purchased from Iranian imported RA5 hot mix asphalt rejuvenator represented by Shanghai Ouduan Industry and Trade Co., Ltd.), Gaoqiao Petrochemical RA5 hot mix asphalt rejuvenator, Jingmen Petrochemical RA5 hot mix asphalt rejuvenator, Jingmen Petrochemical RA25 hot mix asphalt rejuvenator, Sinopec Jinan Branch RA25 hot mix asphalt rejuvenator. Preferably, one or more of Iranian RA5 hot mix asphalt rejuvenator, Gaoqiao RA5 hot mix asphalt rejuvenator, Jingmen RA5 hot mix asphalt rejuvenator, and Jingmen RA25 hot mix asphalt rejuvenator are selected.
[0009] In one or more embodiments of the present invention, the content of cycloalkanes in the cycloalkane oil is not less than 50%, preferably not less than 80%, and is selected from cycloalkane oil 4006, cycloalkane oil 4010, cycloalkane oil 4016, and cycloalkane oil KG16C.
[0010] In one or more embodiments of the present invention, the ring structure of the molecule in the cycloalkyl oil is selected from a monocyclic hydrocarbon group, a linked hydrocarbon group, and a bridged hydrocarbon group.
[0011] In one or more embodiments of the present invention, the thickener is selected from: high melting point polyethylene wax, Fischer-Tropsch wax, amorphous alpha olefin. Preferably, high melting point means a melting point not less than 90°C. Further preferably, the thickener is high melting point polyethylene wax and Fischer-Tropsch wax. Polyethylene wax is selected from: Yimei L103, L108, L203, white wax. Fischer-Tropsch wax is selected from: Future 95# Fischer-Tropsch, Future 115# Fischer-Tropsch, Yitai 85# Fischer-Tropsch, Ningmei 90# Fischer-Tropsch.
[0012] In one or more embodiments of the present invention, the rust inhibitor is selected from: sulfonic acid metal salts, metal soaps and amino compounds. Preferably, the rust inhibitor is selected from: petroleum barium sulfonate and lanolin magnesium soap.
[0013] In one or more embodiments of the present invention, the pour point depressant is selected from: alkyl naphthalene (such as T801), polymethacrylate (such as brand T602HB, T248, SK-8105), polyalphaolefin (such as PAO25, PAO40). Preferably, the pour point depressant is selected from: alkyl naphthalene (such as T801), polymethacrylate (such as brand T602HB, T248, SK-8105).
[0014] In one or more embodiments of the present invention, a method for preparing a wire rope grease comprises the following steps:
[0015] A. Treat the hot mix with asphalt regeneration agent at a constant temperature, then add naphthenic oil and continue stirring;
[0016] B. Add a thickener and continue stirring at a first temperature not lower than the melting point of the material to at least disperse and mix uniformly, and the first temperature is not higher than 200° C.;
[0017] C. Add pour point depressant and rust inhibitor, and continue stirring at a second temperature not lower than the melting point of the material to at least disperse and mix uniformly, and the second temperature is not higher than 200° C.;
[0018] D. Cool down and discharge.
[0019] In one or more embodiments of the present invention, a method for preparing a wire rope grease comprises the following steps:
[0020] A. Treat the hot mix with asphalt regeneration agent at a constant temperature, then add naphthenic oil and continue stirring for 0.5-1h;
[0021] B. Add thickener and stir at 120-130°C for 1-2 hours;
[0022] C. Add pour point depressant and rust inhibitor, and stir at 120-130℃ for 0.5-1h;
[0023] D. Cool down and discharge.
[0024] In one or more embodiments of the present invention, the cooling and discharging is at least any one of the following: cooling to below 85°C to discharging to obtain a solid block product (referring to the environment of room temperature); or cooling to between 85-95°C to discharging to obtain a paste product (referring to the environment of room temperature); or cooling to above 95°C to discharging to obtain a fluid product (referring to the environment of room temperature).
[0025] In one or more embodiments of the present invention, the constant temperature treatment is: maintaining the temperature at 110-130° C. for 1-3 hours.
[0026] Compared with the prior art, the steel wire rope grease and preparation method of the present invention optimizes the formula composition of the grease, uses polar pour point depressants to improve film-forming properties and low-temperature properties, and greatly reduces costs and simplifies processes through raw material screening. It also realizes a steel wire rope grease that can use different cooling processes to obtain different finished product states, so that it can meet the needs of different application scenarios, such as being used both at the production end and in the later operation and maintenance process. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 , a micrograph of an embodiment of the present invention, wherein (a) no pour point depressant is added, and (b) 5% pour point depressant is added;
[0028] Figure 2 , DSC spectrum before and after adding the pour point depressant according to one embodiment of the present invention. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0030] The present invention mainly solves the above problems and provides a preparation scheme, adopts a polar pour point depressant to improve film-forming performance and low-temperature performance, greatly reduces costs and simplifies processes through raw material screening, and adopts different cooling processes to change the finished product state of wire rope grease, so that it can be used at the production end and can also be used in the later operation and maintenance process.
[0031] The raw material base oil used in the wire rope grease of the present invention is a hot mix asphalt regeneration agent with higher viscosity and a cycloalkyl oil, wherein the hot mix asphalt regeneration agent is selected from Iran RA5 hot mix asphalt regeneration agent, Gaoqiao RA5 hot mix asphalt regeneration agent, Jingmen RA5 hot mix asphalt regeneration agent, Jingmen RA25 hot mix asphalt regeneration agent, and Jinan RA25 hot mix asphalt regeneration agent, preferably one or more of Iran RA5 hot mix asphalt regeneration agent, Gaoqiao RA5 hot mix asphalt regeneration agent, Jingmen RA5 hot mix asphalt regeneration agent, and Jingmen RA25 hot mix asphalt regeneration agent. Hot mix asphalt regeneration agent is a product obtained by recycling and reusing waste asphalt and additives through heating, screening, stirring and other process treatments. Compared with base oils such as paraffin oil and extracted oil, it can recycle waste materials, reduce environmental pollution and greatly reduce raw material costs. However, the low-temperature performance of hot mix asphalt regeneration agents of different brands varies greatly, so cycloalkane oil is added to improve the low-temperature performance. The content of cycloalkanes in cycloalkane oil is not less than 50%, and the preferred content is not less than 80%. The structure is preferably one or more of monocyclic hydrocarbons, linked cyclic hydrocarbons and bridged cyclic hydrocarbons. A higher content of cycloalkanes can improve the low-temperature performance on the one hand, and on the other hand, it can also improve the wear resistance, because the molecular chain of straight-chain alkanes will break under the action of large external forces, and the wear resistance is poor. In contrast, due to the ring structure, cycloalkanes have higher strength when the number of carbon atoms is equal.
[0032] The thickener is selected from one or more of high melting point polyethylene wax, Fischer-Tropsch wax, and amorphous alpha olefin, preferably polyethylene wax and Fischer-Tropsch wax, which have good compatibility with wax on the one hand, and can significantly increase the dropping point of the wire rope grease on the other hand, ensuring that it does not slip at higher temperatures.
[0033] The rust inhibitor is selected from sulfonic acid compound metal salts, metal soap compounds and amines, preferably petroleum barium sulfonate and lanolin magnesium soap.
[0034] The pour point depressant is selected from alkyl naphthalene, polymethacrylate, polyalphaolefin, preferably polymethacrylate, which can increase the viscosity and thickening of the wire rope grease on the one hand, and can greatly reduce the pour point of the oil on the other hand, further improving the low temperature performance. In addition, since PMA contains a highly polar ester group, it can be well combined with the metal, and the branched alkane group combines with the wire rope grease to form a stable oil film lubricating layer, which can effectively improve the wear resistance and protection ability.
[0035] The present invention can also obtain products in different states through different cooling processes, which can meet the use requirements of the production end and the maintenance end. The specific scheme can be as follows: stirring and cooling the wire rope grease to below 85°C to obtain a solid block product to meet the production end requirements; stirring and cooling the wire rope grease to between 85-95°C to obtain a paste product, which can meet both the production end requirements and the maintenance end requirements; stirring and cooling the wire rope grease to above 95°C to obtain a fluid product, which can meet the maintenance end requirements. The solid block, paste and fluid states here all refer to states that allow application, not storage states.
[0036] Group 1
[0037] Example 1
[0038] The raw materials of the steel wire rope grease of this embodiment include:
[0039]
[0040]
[0041] The preparation method of the steel wire rope grease of this embodiment comprises the following steps:
[0042] A. Dehydrate the hot mix asphalt regeneration agent at 120℃ for 1 hour, then add naphthenic oil and continue stirring for 0.5 hour;
[0043] B. Add thickener and stir at 120°C for 1 hour;
[0044] C. Add pour point depressant and rust inhibitor, and stir at 120°C for 0.5h;
[0045] D. Stir and cool down, cool to below 70℃, and discharge the material.
[0046] Example 2
[0047] The raw materials of the steel wire rope grease of this embodiment include:
[0048]
[0049] The preparation method of the steel wire rope grease of this embodiment comprises the following steps:
[0050] A. Dehydrate the hot mix asphalt regeneration agent at 120℃ for 1 hour, then add naphthenic oil and continue stirring for 0.5 hour;
[0051] B. Add thickener and stir at 120°C for 1 hour;
[0052] C. Add pour point depressant and rust inhibitor, and stir at 120°C for 0.5h;
[0053] D. Stir and cool down, cool to below 70℃, and discharge the material.
[0054] Example 3
[0055] The raw materials of the steel wire rope grease of this embodiment include:
[0056]
[0057] The preparation method of the steel wire rope grease of this embodiment comprises the following steps:
[0058] A. Dehydrate the hot mix asphalt regeneration agent at 120℃ for 1 hour, then add naphthenic oil and continue stirring for 0.5 hour;
[0059] B. Add thickener and stir at 120°C for 1 hour;
[0060] C. Add pour point depressant and rust inhibitor, and stir at 120°C for 0.5h;
[0061] D. Stir and cool down to 80℃, then discharge the material.
[0062] Comparative Example 1
[0063] The only difference between this comparative example and Example 3 is that no T602HB is added.
[0064] The comparison results of the samples in Example 3 and Comparative Example 1 are as follows: Figure 1 As shown, it is found that the crystallization degree of the sample with added pour point depressant is lower than that without pour point depressant, and the grains are finer and discontinuous. This is because the addition of pour point depressant can precipitate with wax to form eutectic during the cooling process, and the polar groups in the pour point depressant are distributed on the surface of the molecular layer through directional arrangement, which can effectively prevent the growth and connection of wax grains and significantly improve the low temperature performance of the product. When applied on the wire rope, the polar groups have a strong binding ability with the wire rope, so that the wire rope grease can adhere well to the surface of the wire rope, improving the excellent wear resistance, lubrication and rust prevention properties. Figure 2 The difference in the DSC crystallization peaks also further illustrates that the addition of pour point depressants can effectively reduce the crystallinity of wire rope grease.
[0065] Example 4
[0066] The raw materials of the steel wire rope grease of this embodiment include:
[0067]
[0068]
[0069] The preparation method of the steel wire rope grease of this embodiment comprises the following steps:
[0070] A. Dehydrate the hot mix asphalt regeneration agent at 120℃ for 1 hour, then add naphthenic oil and continue stirring for 0.5 hour;
[0071] B. Add thickener and stir at 120°C for 1 hour;
[0072] C. Add pour point depressant and rust inhibitor, and stir at 120°C for 0.5h;
[0073] D. Rapidly cool down to below 80℃ and discharge the material.
[0074] Example 5
[0075] The raw materials of the steel wire rope grease of this embodiment include:
[0076]
[0077] The preparation method of the steel wire rope grease of this embodiment comprises the following steps:
[0078] A. Dehydrate the hot mix asphalt regeneration agent at 120℃ for 1 hour, then add naphthenic oil and continue stirring for 0.5 hour;
[0079] B. Add thickener and stir at 120°C for 1 hour;
[0080] C. Add pour point depressant and stir at 120°C for 0.5h;
[0081] D. Rapidly cool down to below 85℃ and discharge the material.
[0082] Example 6
[0083] The raw materials of the steel wire rope grease of this embodiment include:
[0084]
[0085] The preparation method of the steel wire rope grease of this embodiment comprises the following steps:
[0086] A. Dehydrate the hot mix asphalt regeneration agent at 120℃ for 1 hour, then add cyclohexane oil and continue stirring for 1 hour;
[0087] B. Add thickener and stir at 120°C for 1 hour;
[0088] C. Add pour point depressant and rust inhibitor, and stir at 120°C for 0.5h;
[0089] D. Rapidly cool down to 85℃ and discharge the material.
[0090] Comparative Example 2
[0091] The difference between this comparative example and Example 1 is only that:
[0092] The raw materials of wire rope grease include:
[0093]
[0094]
[0095]
[0096] Group 2
[0097] The difference between Examples 7-12 and Examples 1-6 is that: A. the hot mix asphalt regeneration agent is dehydrated at a constant temperature of 120°C for 1 hour, and then naphthenic oil is added and stirred for 0.5 hours; B. the thickener is added and stirred at a temperature of 120°C for 1 hour;
[0098] C. Add pour point depressant and rust inhibitor, and stir at 120°C for 0.5h;
[0099] D. Rapidly cool down to 95℃ and discharge the material.
[0100]
[0101] Group 3
[0102] The only difference between Examples 13-18 of this group of embodiments and Examples 1-6 is that:
[0103] A. Dehydrate the hot mix asphalt regeneration agent at 120℃ for 1 hour, then add naphthenic oil and continue stirring for 0.5 hour;
[0104] B. Add thickener and stir at 120°C for 1 hour;
[0105] C. Add pour point depressant and rust inhibitor, and stir at 120°C for 0.5h;
[0106] D. Rapidly cool down to 105℃ and discharge the material.
[0107]
[0108]
[0109] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0110] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A wire rope grease, characterized in that: The raw materials include, by weight: Hot mix asphalt regeneration agent: 60-85 parts; Naphthenic oil: 10-30 parts; Thickener: 4-20 parts; Pour point depressant: 1-5 parts; Rust inhibitor: 0-1 part.
2. The wire rope grease according to claim 1, characterized in that: The hot mix asphalt regeneration agent is selected from: Iran RA5 hot mix asphalt regeneration agent, Gaoqiao Petrochemical RA5 hot mix asphalt regeneration agent, Jingmen Petrochemical RA5 hot mix asphalt regeneration agent, Jingmen Petrochemical RA25 hot mix asphalt regeneration agent, and Sinopec Jinan Branch RA25 hot mix asphalt regeneration agent.
3. The wire rope grease according to claim 1, characterized in that: The content of cycloalkanes in the cycloalkane oil is not less than 50%.
4. The wire rope grease according to claim 1, characterized in that: The ring structure of the molecule in the cycloalkyl oil is selected from a monocyclic hydrocarbon group, a linked ring hydrocarbon group and a bridged ring hydrocarbon group.
5. The wire rope grease according to claim 1, characterized in that: The thickener is selected from: high melting point polyethylene wax, Fischer-Tropsch wax, amorphous alpha olefin, wax paste, microcrystalline wax.
6. The wire rope grease according to claim 1, characterized in that: The rust inhibitor is selected from the group consisting of sulfonic acid metal salts, metal soaps and amino compounds.
7. The wire rope grease according to claim 1, characterized in that: The pour point depressant is selected from the group consisting of alkyl naphthalene, polymethacrylate, and poly-alpha olefin.
8. The method for preparing the wire rope grease according to any one of claims 1 to 7, characterized in that: The steps include: A. Dehydrate the hot mix asphalt regeneration agent at a constant temperature, then add naphthenic oil and continue stirring; B. Add a thickener and continue stirring at a first temperature not lower than the melting point of the material to at least disperse and mix uniformly, and the first temperature is not higher than 200° C.; C. Add pour point depressant and rust inhibitor, and continue stirring at a second temperature not lower than the melting point of the material to at least disperse and mix uniformly, and the second temperature is not higher than 200° C.; D. Cool down and discharge.
9. The method for preparing the steel wire rope grease according to claim 8, characterized in that: The cooling and discharging is at least any one of the following: cooling to below 85°C to obtain a solid block product; or cooling to between 85-95°C to obtain a paste product; or cooling to above 95°C to obtain a fluid product.
10. The method for preparing the steel wire rope grease according to claim 8, characterized in that: The constant temperature treatment is: maintaining the temperature at 110-130° C. for 1-3 hours.