Large-wall-thickness X65-grade pipeline steel and manufacturing method thereof

By rationally combining iron, chromium, nickel, niobium and other elements in pipeline steel and using specific processes to form polygonal ferrite + acicular ferrite + granular bainite structure, it solves the problem of high pressure, The problem of insufficient strength and toughness in large flow transportation has improved the reliability and economy of pipelines.

CN118726841AInactive Publication Date: 2024-10-01JIANGSU SHAGANG STEEL CO LTD +2

Patent Information

Application Number
CN202410729529.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing pipeline steel cannot meet the high strength and high toughness requirements in high-pressure, large-flow natural gas transportation environments, and its reliability and economy are insufficient in extreme areas.

Method used

Through reasonable chemical composition combination and process treatment, large-wall-thickness The slab is reheated, rough rolled, finished rolled and other processes to form polygonal ferrite + acicular ferrite + granular bainite-like structure to improve its strength, toughness and weldability.

Benefits of technology

It achieves the high strength, low-temperature toughness and corrosion resistance of pipeline steel, meets the strength requirements for high-pressure and large-flow transportation, and prevents crack initiation and arrest, improving the reliability and economy of the pipeline.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726841A_ABST
    Figure CN118726841A_ABST
Patent Text Reader

Abstract

The invention discloses large-wall-thickness X65-grade pipeline steel and a manufacturing method thereof.The manufacturing method comprises the steps that iron, chromium, nickel, niobium, carbon, silicon, manganese, phosphorus, sulfur, titanium, aluminum, chlorine, potassium and manganese are mixed and heated through a blast furnace, and blast furnace molten iron is obtained; performing KR desulfurization on the blast furnace molten iron; and carrying out steelmaking, refining, vacuum treatment, step-by-step plate blank reheating, rough rolling, finish rolling, cooling, warm straightening, cold straightening, off-line stack cooling, ultrasonic flaw detection and finishing on the blast furnace molten iron subjected to KR desulfurization to obtain the pipeline steel. The steel plate forms a polygonal ferrite, acicular ferrite and granular bainite structure, the drop hammer performance of the steel plate is greatly improved through the structure, high obdurability of the steel plate is guaranteed, and the steel plate can meet the strength requirement for high-pressure and large-flow conveying and the toughness requirement for preventing crack initiation and crack arrest.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a large-wall-thickness X65-grade pipeline steel and a manufacturing method thereof, belonging to the technical field of pipeline steel manufacturing. Background Art

[0002] Today, pipeline steel is mainly used for processing and manufacturing pipelines and pipes for transporting oil and gas. The material of gas pipelines is mainly pipeline steel. With the continuous increase in the use of natural gas in recent years, the development speed of gas pipelines has exceeded the development speed of pipelines for transporting liquids such as oil. However, since most natural gas fields are located in remote areas such as deserts, extremely low permafrost zones and oceans, higher requirements are also placed on the reliability and economy of pipeline steel, such as high strength, high toughness, large deformation, thick wall, high corrosion and good weldability. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the defects of the prior art, provide a large-wall thickness X65 grade pipeline steel and a manufacturing method thereof, and successfully develop a large-wall thickness X65 grade pipeline steel with excellent performance through reasonable chemical composition and process of steel, which is of great significance for the current pipeline construction. The steel plate is formed with polygonal ferrite + acicular ferrite + granular bainite structure, which greatly improves its drop hammer performance and ensures its high strength and toughness, so that it can meet the strength requirements of high-pressure and large-flow transportation and meet the toughness requirements of preventing crack initiation and stopping cracks.

[0004] Preferably, the present invention provides a heavy wall thickness X65 grade pipeline steel, characterized by comprising a homogeneous mixture of iron, chromium, nickel and niobium.

[0005] Preferably, it comprises carbon, silicon, manganese, phosphorus, sulfur, titanium, aluminum, chlorine, potassium and manganese in intimate admixture.

[0006] Preferably, the proportion of chromium is 0.20-0.30%, the proportion of nickel is 0.20-0.25%, and the proportion of niobium is 0.04-0.05%.

[0007] Preferably, the carbon content is 0.03-0.06%, the silicon content is 0.10-0.20%, the manganese content is 1.50-1.65%, the phosphorus content is less than or equal to 0.015%, and the sulfur content is less than or equal to 0.005%.

[0008] Preferably, the proportion of titanium is 0.01-0.02%, the proportion of aluminum is 0.02-0.05%, and the proportion of the mixture of chlorine, potassium and manganese is less than or equal to 0.19%.

[0009] A method for manufacturing a heavy-walled X65 grade pipeline steel, used for manufacturing any of the heavy-walled X65 grade pipeline steels, comprising: Using a blast furnace, iron, chromium, nickel, niobium, carbon, silicon, manganese, phosphorus, sulfur, titanium, aluminum, chlorine, potassium and manganese are mixed and heated to obtain blast furnace iron; Blast furnace hot metal undergoes KR desulfurization; Steelmaking is carried out on blast furnace hot metal after KR desulfurization; Use the refining furnace to fine-tune the molten steel after steelmaking and remove impurities from the molten steel; The molten steel is subjected to a vacuum treatment process to remove hydrogen, nitrogen and inclusions in the molten steel; The molten steel is reheated by a step-by-step slab to obtain a slab; Rough rolling is performed on the slab to obtain a rough-rolled slab; The rough-rolled slab is subjected to finish rolling to obtain a steel plate; The steel plate is subjected to cooling, warm straightening, cold straightening, offline stack cooling, ultrasonic flaw detection and finishing processing to obtain pipeline steel.

[0010] Preferably, the blast furnace hot metal is desulfurized by KR, with a sulfur content of ≤0.005%; After KR desulfurization, the molten iron from the blast furnace enters the 180T top and bottom double-blown converter for steelmaking; The molten steel is subjected to a vacuum treatment process to remove hydrogen, nitrogen and inclusions in the molten steel, with a vacuum degree of <2mbar and hydrogen <2.0ppm.

[0011] Preferably, the molten steel is reheated by a step-by-step slab reheating method to obtain a slab with a cross-section of 320mm×2265mm. The temperature of the preheating section of the slab reheating is controlled at 1000-1150℃, the temperature of the first heating section of the slab reheating is controlled at 1100-1200℃, the temperature of the second heating section of the slab reheating is controlled at 1170-1230℃, the temperature of the soaking section of the slab reheating is controlled at 1170-1220℃, and the time in the furnace is not less than 1.2min / mm.

[0012] Preferably, the rough rolling temperature is controlled at 950-1050°C, and the thickness of the slab after rough rolling is 3.5-5.5 times the thickness of the steel plate. The start temperature of finishing rolling is ≤850℃, the final rolling temperature of the steel plate is controlled at 745±20℃, and the total compression ratio in the finishing rolling stage is ≥70% to obtain the steel plate; Cooling adopts MULPIC accelerated cooling system.

[0013] Preferably, the thickness of the pipeline steel is ≥38mm, the steel grade of the pipeline steel is L450 / X65, the yield strength Rt0.5 of the pipeline steel is between 450 and 600MPa, the tensile strength of the pipeline steel is between 535 and 760MPa, the yield strength ratio of the pipeline steel is ≤0.90, the elongation A50 of the pipeline steel is ≥24%, the average impact energy of the pipeline steel at -30℃ is ≥220J, and the average drop weight shear surface ratio of the pipeline steel at -10℃ is ≥85%.

[0014] The beneficial effects achieved by the present invention are: The present invention successfully develops a thick-walled X65 grade pipeline steel with excellent performance by reasonably involving the chemical composition and process of steel, which is of great significance to the current pipeline construction. The steel plate is formed with polygonal ferrite + acicular ferrite + granular bainite structure, which greatly improves its drop weight performance and ensures its high strength and toughness, so that it can meet the strength requirements of high-pressure and large-flow transportation and meet the toughness requirements of preventing crack initiation and stopping cracks. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0016] Figure 1 It is a schematic diagram of 1 / 4 of the thickness of the pipeline steel head in some embodiments of the present application; Figure 2 is a schematic diagram of 1 / 4 of the thickness of the middle portion of the pipeline steel in some embodiments of the present application; Figure 3 It is a schematic diagram of 1 / 4 of the thickness of the pipeline steel tail in some embodiments of the present application. DETAILED DESCRIPTION

[0017] To facilitate the technical solution of the application, some concepts involved in the application are first explained below.

[0018] See also Figure 1 The present application discloses a thick-walled X65 grade pipeline steel and a manufacturing method thereof, wherein the pipeline steel grade is L450 / X65 grade, and the thickness of the steel plate is ≥38 mm. The manufacturing chemical composition of the thick-walled X65 grade pipeline steel is: C: 0.03~0.06%, Si: 0.10~0.20%, Mn: 1.50~1.65%, P: ≤0.015%, S: ≤0.005%, Cr: 0.20~0.30%, Ni: 0.20~0.25%, Nb: 0.04~0.05%, Ti: 0.01~0.02%, Al: 0.02~0.05%, Pcm≤0.19%, and the rest are iron and unavoidable impurity elements. PCM is a common chemical composition, which is composed of three elements: chlorine, potassium and manganese.

[0019] The manufacturing process includes: configuring steel composition, KR desulfurization, BOF converter, LF refining, RH degassing, CCM continuous casting, slab reheating, rough rolling, intermediate slab waiting for temperature cooling, finishing rolling, accelerated cooling, hot straightening, natural cooling, steel plate warm straightening + cold straightening, offline stack cooling and ultrasonic flaw detection and finishing. The present invention successfully develops a thick-walled X65 grade pipeline steel with excellent performance through reasonable chemical composition and process of steel, which is of great significance for the current pipeline construction. The steel plate is formed with polygonal ferrite + acicular ferrite + granular bainite structure, which greatly improves its drop hammer performance and ensures its high strength and toughness, so that it can meet the strength requirements of high-pressure and large-flow transportation and meet the toughness requirements of preventing crack initiation and stopping cracks.

[0020] Among them, the steel composition is configured: the main role of Cr in steel is to improve the strength and hardness of steel while increasing corrosion resistance. The main role of Ni in steel is to improve strength through solid solution strengthening and refine grains. Under the same strength, it can effectively improve toughness (especially low-temperature toughness) and improve the corrosion resistance of steel. The main role of Nb in steel is to adjust the toughness of steel in a wide range through fine grain strengthening and dispersion strengthening. The addition of niobium can not only improve the strength and toughness of steel, but also improve the high-temperature oxidation resistance and corrosion resistance of steel, reduce the tough-brittle transition temperature of steel, and obtain good weldability and forming performance. At the same time, a lower carbon content is used to ensure its low-temperature toughness.

[0021] KR desulfurization: All blast furnace molten iron can enter the converter blowing process only after it has undergone KR desulfurization, and the S content is ≤0.005%.

[0022] BOF converter: The molten iron after KR desulfurization enters the 180T top and bottom double-blown converter for steelmaking. When the temperature, C, and O meet the process requirements, the molten steel enters the next LF refining process.

[0023] LF / RH refining: LF is mainly used to fine-tune the composition and remove inclusions in the molten steel. When the composition and temperature meet the process requirements, the molten steel is sent to the RH process. RH is a vacuum treatment used to remove H, N and inclusions in the molten steel. The vacuum degree is <2mbar, and H is <2.0ppm.

[0024] The slab reheating adopts step-by-step heating, the slab section is 320mm (thickness) * 2265mm (width), the preheating section temperature is controlled at 1000-1150℃, the first heating section temperature is controlled at 1100-1200℃, the second heating section temperature is controlled at 1170-1230℃, the soaking section temperature is controlled at 1170-1220℃, and the furnace time is not less than 1.2min / mm; In the rough rolling stage, the rough rolling temperature is controlled at 950-1050℃, the intermediate billet thickness after rough rolling is 3.5-5.5 times the thickness of the steel plate, the finishing rolling starting temperature is ≤850℃, the steel plate final rolling temperature is controlled at 745±20℃, and the total compression ratio in the finishing rolling stage is ≥70%; During the steel plate cooling stage, the MULPIC accelerated cooling system is used to adjust the roller speed appropriately according to the actual final cooling conditions so that the final cooling temperature meets the requirements.

[0025] The pipeline steel has a thickness of ≥38 mm, a steel grade of L450 / X65, a yield strength Rt0.5 of 450~600 MPa, a tensile strength Rm of 535~760 MPa, a yield strength ratio of ≤0.90, and an elongation A50 of ≥24%. The average impact energy at -30°C is ≥220 J, and the average shear ratio of the drop hammer at -10°C is ≥85%.

[0026] In summary, the heavy-walled X65 grade pipeline steel and its manufacturing method of the present invention successfully develop heavy-walled X65 grade pipeline steel with excellent performance through reasonable chemical composition and process of steel, which is of great significance to the current pipeline construction.

[0027] The microstructure photos of the steel plates produced by this method are as follows: Figures 1 to 3 As shown. Taking 32mm X65M as an example, the process route is: configuration of steel grade composition, KR desulfurization, BOF converter, LF refining, RH degassing, CCM continuous casting, slab reheating, rough rolling, intermediate billet waiting for temperature cooling, finishing rolling, accelerated cooling, hot straightening, natural cooling, steel plate warm straightening + cold straightening, offline stack cooling and ultrasonic flaw detection, finishing, size verification, steel plate marking, and storage. The smelting furnace of the embodiment is shown in Table 1, the rolling process of the mother plate of the embodiment is shown in Table 2, and the mechanical properties of the mother plate of the embodiment are shown in Table 3.

[0028] Table 1: Smelting furnaces of the embodiment

[0029] Table 2: Example motherboard rolling process

[0030] Table 3: Mechanical properties of motherboard in the examples

[0031] SA refers to the shear surface ratio of the drop hammer fracture. From the metallographic point of view, the steel plate is formed into a polygonal ferrite + acicular ferrite + granular bainite structure, which greatly improves its drop hammer performance and ensures its high strength and toughness, so that it can meet the strength requirements of high-pressure and large-flow transportation and meet the toughness requirements of preventing crack initiation and crack arrest.

[0032] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0033] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention invented herein. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not invented by the present invention. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.

[0034] The above specific implementation methods further illustrate the purpose, technical solutions and beneficial effects of the present application in detail. It should be understood that the above are only specific implementation methods of the present application and are not used to limit the protection scope of the present application. Any modifications, equivalent substitutions, improvements, etc. made on the basis of the technical solutions of the present application should be included in the protection scope of the present application.

Claims

1. A thick wall X65 grade pipeline steel, characterized in that: It consists of a uniform mixture of iron, chromium, nickel and niobium.

2. The thick-walled X65 grade pipeline steel according to claim 1, characterized in that: It includes a uniform mixture of carbon, silicon, manganese, phosphorus, sulfur, titanium, aluminum, chlorine, potassium and manganese.

3. The thick-walled X65 grade pipeline steel according to claim 1, characterized in that: The proportion of chromium is 0.20~0.30%, the proportion of nickel is 0.20~0.25%, and the proportion of niobium is 0.04~0.05%.

4. The thick-walled X65 grade pipeline steel according to claim 2, characterized in that: The proportion of carbon is 0.03~0.06%, the proportion of silicon is 0.10~0.20%, the proportion of manganese is 1.50~1.65%, the proportion of phosphorus is less than or equal to 0.015%, and the proportion of sulfur is less than or equal to 0.005%.

5. The thick-walled X65 grade pipeline steel according to claim 2, characterized in that: The proportion of titanium is 0.01~0.02%, the proportion of aluminum is 0.02~0.05%, and the mixture of chlorine, potassium and manganese is less than or equal to 0.19%.

6. A method for manufacturing thick-walled X65 grade pipeline steel, characterized in that: Used to manufacture the heavy-walled X65 grade pipeline steel according to any one of claims 1 to 5, comprising: Using a blast furnace, iron, chromium, nickel, niobium, carbon, silicon, manganese, phosphorus, sulfur, titanium, aluminum, chlorine, potassium and manganese are mixed and heated to obtain blast furnace iron; Blast furnace hot metal undergoes KR desulfurization; Steelmaking is carried out on blast furnace hot metal after KR desulfurization; Use the refining furnace to fine-tune the molten steel after steelmaking and remove impurities from the molten steel; The molten steel is subjected to a vacuum treatment process to remove hydrogen, nitrogen and inclusions in the molten steel; The molten steel is reheated by a step-by-step slab to obtain a slab; Rough rolling is performed on the slab to obtain a rough-rolled slab; The rough-rolled slab is subjected to finish rolling to obtain a steel plate; The steel plate is subjected to cooling, warm straightening, cold straightening, offline stack cooling, ultrasonic flaw detection and finishing processing to obtain pipeline steel.

7. The method for manufacturing a thick-walled X65 grade pipeline steel according to claim 6, characterized in that: The blast furnace hot metal is desulfurized by KR, and the sulfur content is ≤0.005%; The molten iron from the blast furnace after KR desulfurization enters the 180T top and bottom double-blown converter for steelmaking; The molten steel is subjected to a vacuum treatment process to remove hydrogen, nitrogen and inclusions in the molten steel, with a vacuum degree of <2mbar and hydrogen <2.0ppm.

8. The method for manufacturing a thick-walled X65 grade pipeline steel according to claim 6, characterized in that: The molten steel is reheated by a step-by-step slab reheating method to obtain a slab with a cross-section of 320mm×2265mm. The temperature of the preheating section of the slab reheating is controlled at 1000-1150°C, the temperature of the first heating section of the slab reheating is controlled at 1100-1200°C, the temperature of the second heating section of the slab reheating is controlled at 1170-1230°C, the temperature of the soaking section of the slab reheating is controlled at 1170-1220°C, and the time in the furnace is not less than 1.2min / mm.

9. The method for manufacturing a thick-walled X65 grade pipeline steel according to claim 6, characterized in that: The rough rolling temperature is controlled at 950-1050℃, and the thickness of the slab after rough rolling is 3.5-5.5 times the thickness of the steel plate. The start temperature of finishing rolling is ≤850℃, the final rolling temperature of the steel plate is controlled at 745±20℃, and the total compression ratio in the finishing rolling stage is ≥70% to obtain the steel plate; Cooling adopts MULPIC accelerated cooling system.

10. The method for manufacturing a thick-walled X65 grade pipeline steel according to claim 6, characterized in that: The thickness of the pipeline steel is ≥38mm, the steel grade of the pipeline steel is L450 / X65, the yield strength Rt0.5 of the pipeline steel is between 450 and 600MPa, the tensile strength of the pipeline steel is between 535 and 760MPa, the yield strength ratio of the pipeline steel is ≤0.90, the elongation A50 of the pipeline steel is ≥24%, the average impact energy of the pipeline steel at -30℃ is ≥220J, and the average drop weight shear surface ratio of the pipeline steel at -10℃ is ≥85%.

Citation Information

Patent Citations

  • Hot-rolled steel plate for coal slurry conveying pipe and manufacturing method thereof

    CN102676949A

  • Panel for thick wall tempering deep sea pipeline and production method thereof

    CN107988558A

  • Production method of improving surface quality of low-steel-grade pipeline steel

    CN110016626A

  • X65 pipeline steel and manufacturing method thereof

    CN110306112A

  • Method for producing X65 acid-resistant pipeline steel plate used under low-cost and ultralow-temperature conditions through curling furnace

    CN112410647A

Cited By

  • Anti-crack marine riser X65M steel plate and production method thereof

    CN122279397A