Method for rapidly detecting delta phase in steel-copper-tin-bismuth alloy shaft sleeve

By using the methods of cutting, inlaying, rough grinding, fine grinding, polishing and microhardness measurement in metallographic testing, the problem of difficulty in distinguishing δ phase and Bi phase in the existing technology is solved, and the detection of copper-tin-bismuth alloy shafts is realized. The accurate detection of δ phase in the sleeve improves the detection efficiency and accuracy.

CN118731019APending Publication Date: 2024-10-01YANGZHOU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410892092.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to accurately distinguish between the delta phase and the Bi phase in copper-tin-bismuth alloys during metallographic testing with existing technology, leading to errors in mechanical performance judgment and affecting product qualification rates and production costs.

Method used

A rapid detection method is adopted, including cutting, inlaying, rough grinding, fine grinding, polishing, optical microscope observation and microhardness measurement, and absolute alcohol is used instead of polishing paste and Image pro plus software is used to determine the δ phase content to ensure accurate differentiation and Determine the delta phase.

Benefits of technology

The accurate detection of the δ phase in the copper-tin-bismuth alloy bushing is achieved, the detection efficiency and accuracy are improved, the misjudgment rate is reduced, and the accuracy of the mechanical property judgment of the alloy is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731019A_ABST
    Figure CN118731019A_ABST
Patent Text Reader

Abstract

The invention discloses a method for rapidly detecting a delta phase in a steel-copper-tin-bismuth alloy shaft sleeve, which comprises the steps of cutting, inlaying, coarse grinding, accurate grinding, polishing, optical microscopic observation, microhardness measurement and delta phase content determination. A relatively smooth delta-phase light gray area in the irregular Bi-phase gray area is distinguished through microscope observation, and the delta-phase light gray area is further subjected to microhardness measurement to confirm the content of the delta phase, so that whether the copper-tin-bismuth-containing alloy shaft sleeve product with the steel backing is qualified or not is judged. Whether the delta phase exists in the copper-tin-bismuth alloy shaft sleeve or not and the content of the delta phase can be accurately judged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallographic sample detection, and in particular relates to a method for quickly detecting a delta phase in a steel-copper-tin-bismuth alloy shaft sleeve. Background Art

[0002] Copper-tin alloys are widely used in the production of automotive bushings. In the field of testing, metallographic testing of tin-bronze alloys is required. Sample preparation is one of the necessary steps in metallographic testing. The usual sample preparation steps are rough grinding, fine grinding and polishing. According to the copper-tin binary alloy phase diagram analysis, in the actual production process, when the tin content is greater than or equal to 11%, there is a brittle and hard δ phase in the tin-bronze alloy, which will greatly affect the mechanical properties of the copper-tin alloy. Although the overall tin content is less than 11% through component analysis, an indefinite amount of δ phase will still precipitate in the alloy during the production process due to heating temperature, cooling rate, uneven powder spreading and other reasons. Bismuth, as an element insoluble in copper, will precipitate along the grain boundaries of the copper matrix phase. These δ phases are interspersed in the Bi phase that is insoluble in Cu, and are difficult to observe under a light microscope using traditional sample preparation methods. In traditional routine testing, after polishing with polishing paste, the sample is observed under a metallographic microscope to see if there is a δ phase. The inventors found that: in the actual metallographic preparation, the microscopic morphology of the sample, such as Figure 3 In (a), only the darker irregular area exists, and it is impossible to distinguish the Bi phase and the δ phase, or even whether there is a hole. Therefore, it is often passed as a qualified product, and the alloy performance cannot be correctly judged, which will lead to a reduction in the tool life during the cutting process of the copper-tin-bismuth alloy, resulting in a lower product qualification rate and increased production costs. Summary of the invention

[0003] Purpose of the invention: In order to solve the technical problems existing in the prior art, the present invention provides a method for quickly detecting the δ phase in a steel-copper-tin-bismuth alloy sleeve, which can accurately determine whether the δ phase exists in the copper-tin-bismuth alloy sleeve and its content.

[0004] Technical solution: To achieve the above invention purpose, the present invention adopts the following technical solution: A method for quickly detecting the δ phase in a steel-copper-tin-bismuth alloy sleeve, comprising the following steps: S1, cutting: cutting the sleeve into slice samples of appropriate size; S2, Metallographic Preparation: (1) Mounting: Place the copper-tin-bismuth alloy surface downward in a mounting machine, introduce bakelite powder and heat to mount it, and obtain a columnar specimen with a size of not less than φ20 mm × 8~10 mm; (2) Rough grinding: Use 80#Sic sandpaper for rough grinding to ensure that the sample is flat without curvature or depression; (3) Fine grinding: Use 200#Sic, 400#Sic, 600#Sic, 800#Sic, 1000#Sic, and 1200#Sic sandpapers to fine grind until there are no obvious wear marks on the surface of the sample; (4) Polishing: The finely ground sample is sent to a grinder and polisher, and polished with a black navy mud polishing cloth at a speed of 600-700 r / min and a pressure of 5-25 g. During the polishing process, alcohol with a purity of more than 99.9% is used as a cooling lubricant instead of polishing paste, and the polishing time is controlled not to exceed 5 s. S3, optical microscope observation: observe under an optical microscope at a magnification of 400 times or more. If no copper-bismuth phase boundary is found, repeat the polishing step until a clear copper-bismuth phase boundary can be clearly observed and proceed to the next step; S4, microhardness measurement: select all relatively smooth areas on the copper-bismuth phase boundary for microhardness measurement. If the microhardness is less than 250HV, it indicates that there is no δ phase, indicating that the sleeve meets the processing requirements; if there is an area with a microhardness ≥ 250HV, there is a δ phase on the surface, and proceed to the next step; S5, use Image pro plus software to measure the δ phase content. If the δ phase content is greater than 5%, it means that the sleeve does not meet the processing requirements; if the δ phase content is ≤5%, it means that the sleeve meets the processing requirements and is completed.

[0005] Furthermore, in step S3, the magnification of the optical microscope is 500 times.

[0006] Furthermore, the size of the sliced ​​sample in step S1 is controlled within 10 mm×10 mm.

[0007] Beneficial effect: Compared with the prior art which conventionally uses polishing paste for polishing and then directly confirms the presence of δ phase through microscopic observation, which is very easy to make misjudgment, the present invention uses anhydrous alcohol instead of polishing paste and can accurately distinguish and judge the presence of δ phase and determine the δ phase content through microhardness test. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 The figure is a schematic flow chart of the method for rapidly detecting the δ phase in a steel-copper-tin-bismuth alloy bushing according to the present invention.

[0009] Figure 2 Phase diagram of copper-tin binary alloy.

[0010] Figure 3 The test results of the metallographic samples obtained by conventional metallographic preparation methods are as follows: (a) is the micromorphology diagram; (b) is the microhardness diagram; and (c) is the δ phase analysis result.

[0011] Figure 4The metallographic sample test results obtained by the method of the present invention are as follows: (a) is a microscopic morphology diagram; (b) is a microhardness diagram; and (c) is a delta phase analysis result.

[0012] Figure 5 The microscopic morphology of the metallographic sample obtained by the method of the present invention at a magnification of 500 times is shown.

[0013] Figure 6 The microscopic morphology of the metallographic sample obtained by the method of the present invention at a magnification of 200 times is shown. DETAILED DESCRIPTION

[0014] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0015] First, the bismuth-containing copper-tin alloy sleeve of the steel back is cut to obtain a sample of suitable size. The cutting requirement is: the sample size is controlled within 10×10 mm. Example

[0016] (1) The sample was obtained and inlaid in an inlaying machine by bakelite powder inlaying. The sample size was φ20 mm × 8 mm.

[0017] (2) Use 80#Sic sandpaper to grind the alloy surface until it is smooth.

[0018] (3) Get sandpaper with mesh sizes of 200#Sic, 400#Sic, 600#Sic, 800#Sic, 1000#Sic, and 1200#Sic for fine grinding. Each time the sandpaper mesh size is changed, the sample needs to be rotated 90 degrees to continue grinding (to better observe and confirm whether the wear marks of the previous sandpaper mesh size are completely covered). Make sure that the wear marks of the previous sandpaper are removed before changing to a finer sandpaper until there are no obvious wear marks on the surface, and then proceed to the next step. This grinding process does not require the use of lubrication / coolant.

[0019] (4) Place the sample on one side of the center of the grinder and polisher, adjust the speed of the grinder and polisher to 650 r / min, control the pressure at 10 g, use a black navy nylon polishing cloth, use water and a polishing paste with a particle size of 2.5w for polishing, and the polishing time is 5 s.

[0020] (5) After polishing, clean the alloy surface with alcohol and blow dry with a hair dryer.

[0021] (6) Place it under a 500x optical microscope for observation. Figure 3As shown in (a), in addition to the gray area of ​​the copper matrix, there are also black irregular areas in the micrograph. It is impossible to determine whether the black irregular areas are holes, Bi phases or δ phases, and the microscopic morphology after polishing cannot be distinguished.

[0022] (7) Use a microhardness tester to measure the microhardness with a load of 25N and a load duration of 10s. The results are as follows: Figure 3 As shown in (b) in .

[0023] (8) Image pro plus 6.0 software was used to determine the microstructure content greater than 250HV. The results are as follows: Figure 3 As shown in (c) in .

[0024] (9) The results showed that the metallographic structure was not clearly displayed, making it difficult to distinguish the true microstructure; the test force was too large and the load was maintained for too long. Due to the influence of the steel back, the overall hardness was too high, resulting in incorrect content calculation and a large error. Ultimately, it was difficult to correctly determine the processing performance of the copper-tin-bismuth bushing. Example

[0025] (1) The sample was obtained and inlaid in an inlaying machine by bakelite powder inlaying. The sample size was φ20 mm × 8 mm.

[0026] (2) Use 80#Sic sandpaper to grind the alloy surface until it is smooth.

[0027] (3) Get sandpaper with mesh sizes of 200#Sic, 400#Sic, 600#Sic, 800#Sic, 1000#Sic, and 1200#Sic for fine grinding. Each time the sandpaper mesh size is changed, the sample needs to be rotated 90 degrees to continue grinding (to better observe and confirm whether the wear marks of the previous sandpaper mesh size are completely covered). Make sure that the wear marks of the previous sandpaper are removed before changing to a finer sandpaper until there are no obvious wear marks on the surface, and then proceed to the next step. This grinding process does not require the use of lubricants / coolants. This grinding process does not require the use of lubricants / coolants.

[0028] (4) Place the sample on one side of the center of the grinder and polisher, adjust the speed of the grinder and polisher to 650 r / min, control the pressure at 10 g, use a black navy nylon polishing cloth, and polish with 99.9% alcohol for 5 seconds.

[0029] (5) After polishing, clean the alloy surface with alcohol and blow dry with a hair dryer.

[0030] (6) Place it under a 500x optical microscope for observation. Figure 4 As shown in (a) in .

[0031] (7) Use a microhardness tester to measure the microhardness with a load of 10N and a load duration of 5s. The results are as follows: Figure 4 As shown in (b) in .

[0032] (8) Image pro plus 6.0 software was used to determine the microstructure content greater than 250HV. The results are as follows: Figure 4 As shown in (c) in .

[0033] (9) This scheme can clearly identify the boundary of the δ phase included in Bi, providing a clear microstructure for the measurement of microhardness. Lower load force and load holding time can more accurately measure the microhardness of the δ phase, thereby better judging the processing performance of the copper-tin-bismuth bushing. Figure 5 This is a metallographic microscopic image at 500 times magnification. Figure 5 It can be seen that the black spots are metal holes, the Bi phase precipitates along the phase grain boundaries in the copper matrix and appears as irregular gray areas, and light gray circular spots appear in the gray areas, which are suspected to be δ phase areas, and microhardness testing is needed for further confirmation.

[0034] In addition, the inventors also found that steel is used as the steel back during the production process of the sleeve, and the hardness of the copper alloy itself is relatively low. Therefore, in the process of judging the mechanical properties of the alloy by measuring the δ phase content based on microhardness, if the operation is improper, the overall microhardness will be too high, thereby affecting the judgment of the mechanical processing performance of the sleeve. Therefore, in the present invention, after distinguishing the Bi phase and the suspected δ phase by microhardness, the hardness of the δ phase in the light gray area is generally more than 250HV, while the hardness of the Bi phase is lower than 250HV, which is further confirmed. Due to the preliminary confirmation of the δ phase, the area that needs to measure the microhardness is saved, which greatly improves the detection efficiency. Figure 6 The magnification is 200 times, and the δ phase region is barely distinguishable.

[0035] The above descriptions are only some embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for rapidly detecting the delta phase in a steel-copper-tin-bismuth alloy sleeve, characterized in that The following steps are involved: S1, cutting: cutting the sleeve into slice samples of appropriate size; S2, Metallographic Preparation: (1) Mounting: Place the copper-tin-bismuth alloy surface downward in a mounting machine, introduce bakelite powder and heat to mount it, and obtain a columnar specimen with a size of not less than φ20 mm × 8~10 mm; (2) Rough grinding: Use 80#Sic sandpaper for rough grinding to ensure that the sample is flat without curvature or depression; (3) Fine grinding: Use 200#Sic, 400#Sic, 600#Sic, 800#Sic, 1000#Sic, and 1200#Sic sandpapers to fine grind until there are no obvious wear marks on the surface of the sample; (4) Polishing: The finely ground sample is sent to a grinder and polisher, and polished with a black navy mud polishing cloth at a speed of 600-700 r / min and a pressure of 5-25 g. During the polishing process, alcohol with a purity of more than 99.9% is used as a cooling lubricant instead of polishing paste, and the polishing time is controlled not to exceed 5 s. S3, optical microscope observation: observe under an optical microscope at a magnification of 400 times or more. If no copper-bismuth phase boundary is found, repeat the polishing step until a clear copper-bismuth phase boundary can be clearly observed and proceed to the next step; S4, microhardness measurement: select all relatively smooth areas on the copper-bismuth phase boundary for microhardness measurement. If the microhardness is less than 250HV, it indicates that there is no δ phase, indicating that the sleeve meets the processing requirements; if there is an area with a microhardness ≥ 250HV, there is a δ phase on the surface, and proceed to the next step; S5, use Image pro plus software to measure the δ phase content. If the δ phase content is greater than 5%, it means that the sleeve does not meet the processing requirements; if the δ phase content is ≤5%, it means that the sleeve meets the processing requirements and is completed.

2. The method for rapidly detecting the δ phase in a steel-copper-tin-bismuth alloy sleeve according to claim 1, characterized in that: The magnification of the optical microscope in step S3 is 500 times.

3. The method for rapidly detecting the δ phase in a steel-copper-tin-bismuth alloy sleeve according to claim 1, characterized in that: In step S1, the size of the sliced ​​sample is controlled within 10 mm×10 mm.

Citation Information

Cited By

  • Method for inlaying and detecting micron coating sample

    CN119375003A